Barium-Calcium Ferrite Disc Magnet: 0.09 mol BaCO3 and 0.01 mol CaCO3 (Went, Philips 1956, Ex. 19)

A ceramic magnet with a tenth of the barium replaced by calcium: 0.09 mol barium carbonate and 0.01 mol calcium carbonate to 0.6 mol iron oxide, made as in Example 18: milled, presintered at 1000 °C, milled again, formed and passed through a 1330 °C furnace in 10 minutes. Went's rod held 1,705 gauss with a coercive force of 1,110 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 19. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Juu
2 days

Maagizo

1

Weigh barium carbonate, chalk and iron oxide

Weigh 17.76 g barium carbonate (0.09 mol), 1.001 g calcium carbonate (0.01 mol) and 95.55 g ferric oxide (0.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Vifaa kwa hatua hii:

Kabonati ya bariamu (witherite)Kabonati ya bariamu (witherite)17.76 g
Kaboneti ya kalsiamu (chaki nyeupe)Kaboneti ya kalsiamu (chaki nyeupe)1.001 g
Oksidi ya feriOksidi ya feri95.55 g

Zana zinazohitajika:

Mizani ya mizani-mbiliMizani ya mizani-mbili
Glavu za mpiraGlavu za mpira
Kinga ya Kupumua ya P100Kinga ya Kupumua ya P100
2

Mill with alcohol 4 hours, dry at 150 °C

Grind with alcohol in a ball mill for 4 hours and dry in air at 150 °C.

Zana zinazohitajika:

Kinu cha mipira ya chumaKinu cha mipira ya chuma
Etanoli ya maabara, 95 %Etanoli ya maabara, 95 %
Tanuri la kukaushiaTanuri la kukaushia
3

Presinter in air at 1000 °C for 2 hours

Fire in air at 1000 °C for 2 hours.

Zana zinazohitajika:

Tanuri ya muffleTanuri ya muffle
Kikaango cha kuyeyushia chenye mfuniko (kaure)Kikaango cha kuyeyushia chenye mfuniko (kaure)
Koleo la kaure ya kuyeyushiaKoleo la kaure ya kuyeyushia
Glavu Zinazostahimili JotoGlavu Zinazostahimili Joto
4

Mill again 4 hours, dry, form

Grind again with alcohol for 4 hours and dry. Example 19 extrudes a rod; ours: press discs at 1.5 tonnes per cm², as Example 18 moulds its rod.

Zana zinazohitajika:

Kinu cha mipira ya chumaKinu cha mipira ya chuma
Etanoli ya maabara, 95 %Etanoli ya maabara, 95 %
Tanuri la kukaushiaTanuri la kukaushia
Mashine ya kubana ya haidrolikiMashine ya kubana ya haidroliki
Kalibu ya kubana diskiKalibu ya kubana diski
5

Pass through a 1330 °C zone in 10 minutes

Sinter at 1330 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Zana zinazohitajika:

Tanuru ya MrijaTanuru ya Mrija
Glavu Zinazostahimili JotoGlavu Zinazostahimili Joto
6

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Zana zinazohitajika:

Sumaku ya umemeSumaku ya umeme
DiraDira

Vifaa

3

Zana Zinazohitajika

15

Blueprint zinazohusiana

Blueprint hizi zinashiriki maarifa — mbinu, vifaa au kanuni

CC0 Umma Wote

Mchoro huu umetolewa chini ya CC0. Uko huru kunakili, kubadilisha, kusambaza, na kutumia kazi hii kwa madhumuni yoyote, bila kuomba ruhusa.

Saidia Mtengenezaji kwa kununua bidhaa kupitia Mchoro wao ambapo wanapata Kamisheni ya Mtengenezaji iliyowekwa na Wachuuzi, au unda marudio mapya ya Mchoro huu na uiunganishe kama kiungo katika Mchoro wako kuchangia mapato.

Majadiliano

(0)

Ingia kujiunga na majadiliano

Inapakia maoni...