Barium Ferrite Disc Magnet from Natural Magnetite, Presintered at 900 °C (Went, Philips 1956, Ex. 36, Procedure 1)
Charlie

Imeundwa na

Charlie

28. Oktoba 2026DE
2
0
0
0
0

Barium Ferrite Disc Magnet from Natural Magnetite, Presintered at 900 °C (Went, Philips 1956, Ex. 36, Procedure 1)

A barium ferrite magnet made from natural magnetite instead of ferric oxide: barium carbonate and magnetite ground 18 hours, presintered 3 hours at 900 °C, ground again 18 hours, pressed and sintered 2 hours at 1200 °C. Went's rod held 1,450 gauss with a coercive force of 2,425 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 36. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Juu
2 days

Maagizo

1

Weigh barium carbonate and magnetite

Weigh 9.9 g barium carbonate (0.05 mol) and 46.9 g natural magnetite, Fe3O4 (0.20 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Vifaa kwa hatua hii:

Kabonati ya bariamu (witherite)Kabonati ya bariamu (witherite)9.9 g
MagnetitiMagnetiti46.9 g

Zana zinazohitajika:

Mizani ya mizani-mbiliMizani ya mizani-mbili
Glavu za mpiraGlavu za mpira
Kinga ya Kupumua ya P100Kinga ya Kupumua ya P100
2

Grind 18 hours in a ball mill

Grind the mixture in a ball mill for 18 hours. The patent does not say whether wet or dry.

Zana zinazohitajika:

Kinu cha mipira ya chumaKinu cha mipira ya chuma
Kinga ya Kupumua ya P100Kinga ya Kupumua ya P100
3

Presinter at 900 °C for 3 hours

Fire the ground mixture at 900 °C for three hours and let it cool.

Zana zinazohitajika:

Tanuri ya muffleTanuri ya muffle
Kikaango cha kuyeyushia chenye mfuniko (kaure)Kikaango cha kuyeyushia chenye mfuniko (kaure)
Koleo la kaure ya kuyeyushiaKoleo la kaure ya kuyeyushia
Glavu Zinazostahimili JotoGlavu Zinazostahimili Joto
4

Grind 18 hours in a ball mill

Grind it again in a ball mill for 18 hours. The patent does not say whether wet or dry.

Zana zinazohitajika:

Kinu cha mipira ya chumaKinu cha mipira ya chuma
Kinga ya Kupumua ya P100Kinga ya Kupumua ya P100
5

Press at 1.5 t/cm²

Press at 1.5 tonnes per cm² (ours: discs instead of a rod).

Zana zinazohitajika:

Mashine ya kubana ya haidrolikiMashine ya kubana ya haidroliki
Kalibu ya kubana diskiKalibu ya kubana diski
6

Sinter at 1200 °C for 2 hours

Sinter at 1200 °C for 2 hours. The patent gives no atmosphere for this example. Went's rod: 1,450 gauss, 2,425 oersted.

Zana zinazohitajika:

Tanuri ya muffleTanuri ya muffle
Koleo la kaure ya kuyeyushiaKoleo la kaure ya kuyeyushia
Glavu Zinazostahimili JotoGlavu Zinazostahimili Joto
7

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Zana zinazohitajika:

Sumaku ya umemeSumaku ya umeme
DiraDira

Vifaa

2

Zana Zinazohitajika

12

Blueprint zinazohusiana

Blueprint hizi zinashiriki maarifa — mbinu, vifaa au kanuni

CC0 Umma Wote

Mchoro huu umetolewa chini ya CC0. Uko huru kunakili, kubadilisha, kusambaza, na kutumia kazi hii kwa madhumuni yoyote, bila kuomba ruhusa.

Saidia Mtengenezaji kwa kununua bidhaa kupitia Mchoro wao ambapo wanapata Kamisheni ya Mtengenezaji iliyowekwa na Wachuuzi, au unda marudio mapya ya Mchoro huu na uiunganishe kama kiungo katika Mchoro wako kuchangia mapato.

Majadiliano

(0)

Ingia kujiunga na majadiliano

Inapakia maoni...