Extruded polystyrene foam blown with a propylene gas fraction instead of methyl chloride. Polystyrene stands two days at 40 °C with the propylene under pressure and becomes a gel. Let out at 60 °C (300 psi in the tower), it swelled into a log 11 inches across, weighing 3.08 lb per cubic foot, with small uniform cells. Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 3. Picture: the patent's drawing.
Juu
3 days

Maagizo

1

Charge the tower with polystyrene

Charge a high-pressure tower with 300 lb of granular polystyrene.

Vifaa kwa hatua hii:

PolistiriniPolistirini300 paundi

Zana zinazohitajika:

Riakta ya shinikizoRiakta ya shinikizo
Mizani ya mizani-mbiliMizani ya mizani-mbili
Glavu za mpiraGlavu za mpira
2

Add the propylene fraction

Add 100 lb of a cracked-oil gas fraction that is about 93 % propylene, under pressure, and close the tower. Propylene is a flammable gas: no flames, strong ventilation.

Vifaa kwa hatua hii:

PropiliniPropilini100 paundi

Zana zinazohitajika:

Mtungi wa gesi yenye shinikizoMtungi wa gesi yenye shinikizo
Riakta ya shinikizoRiakta ya shinikizo
Miwani ya kinga dhidi ya kemikaliMiwani ya kinga dhidi ya kemikali
3

Stand two days at 40 °C

Let the tower stand for two days at 40 °C while the polystyrene takes up the propylene.

Zana zinazohitajika:

Riakta ya shinikizoRiakta ya shinikizo
Kipimajoto cha maabaraKipimajoto cha maabara
4

Let it out at 60 °C

Open the valved outlet near the bottom (2.5 inch in the patent) at 60 °C. The pressure is about 300 psi. The gel flows out and swells into a log 11 inches across, 3.08 lb per cubic foot, with small uniform cells. Close the outlet again. The patent heated step by step (50, 60, 75 °C) for several hours each, letting a portion out at each step.

Zana zinazohitajika:

Riakta ya shinikizoRiakta ya shinikizo
Kipimajoto cha maabaraKipimajoto cha maabara
Miwani ya kinga dhidi ya kemikaliMiwani ya kinga dhidi ya kemikali
Glavu za mpiraGlavu za mpira
5

Saw into boards

When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).

Zana zinazohitajika:

Msumeno wa useremalaMsumeno wa useremala
Glavu za mpiraGlavu za mpira

Vifaa

2
  • 300 paundi
    Kishikilia Nafasi
  • 100 paundi
    Kishikilia Nafasi

Zana Zinazohitajika

7

CC0 Umma Wote

Mchoro huu umetolewa chini ya CC0. Uko huru kunakili, kubadilisha, kusambaza, na kutumia kazi hii kwa madhumuni yoyote, bila kuomba ruhusa.