Ferromolybdenum: Molybdic Oxide Smelted with Coke and Lime into Molten Steel in an Electric Arc Furnace (Brigham, US 4,160,661)
Technical molybdic oxide is fed in cans, with coke and lime, into a bath of molten steel in a 3000 kVA arc furnace. The electrodes stay in the slag, and the coke is trimmed after every charge unit so the metal keeps under 0.1 % carbon. Ferrosilicon and lime strip the slag, and the metal is shotted in running water.
Result: from 5000 lb oxide, 3110 lb shot and pig of 54.1 % molybdenum, 0.06 % carbon, 43.1 % iron (Heat 4), using 1.94 kWh per lb of molybdenum.
Source: Brigham, Sirianni and Garner, US patent 4,160,661 (1979), Example 2, Heat 4. Not given: how the shot was heated while drying overnight. Picture drawn by Youblob.
Juu
1 day
Maagizo
1
1
Melt the steel
Melt the steel
In a three-phase 3000 kVA arc furnace with 8 in graphite electrodes, lined with magnesia brick and rammed basic refractory (about 60 % MgO), 5 ft 6 in across and 26 in deep below the tap hole, melt 812 lb steel plate with 80 lb burnt lime under full power. Lead the fume to a bag house.
Vifaa kwa hatua hii:
Bamba la chuma laini812 paundiZana zinazohitajika:
Chokaa hai
Tanuru la tao la umeme
Elektrodi ya grafiti
Chumba cha vichujio vya mifuko2
2
Make up the charge units
Make up the charge units
While it melts, weigh out five charge units, each 1000 lb molybdic oxide (in cans of 37 lb oxide in a 2 lb steel can), 250 lb coke and 320 lb lime. For Heat 4 that was 5000 lb oxide, 1150 lb coke, 1600 lb lime and 1488 lb steel in plate and cans. Ours: metallurgical coke for the dried breeze coke.
Vifaa kwa hatua hii:
Oksidi ya molibdeni ya kiufundi5000 paundi
Bamba la chuma laini1488 paundiZana zinazohitajika:
Kokoo ya kutengeneza chuma
Chokaa hai
Mizani ya jukwaa ya kiwanda3
3
Smelt in the bath
Smelt in the bath
When the bath is molten at about 1450 °C, add one can of oxide with equal shovels of coke and lime every 2 minutes, about 1 hour per unit. Use the 205 V tap so the electrodes dip only into the slag; hold the bath at most 1760 °C. About 1 kWh per lb of oxide.
Zana zinazohitajika:
Sepetu
Tanuru la tao la umeme4
4
Keep the carbon down
Keep the carbon down
After every charge unit, dip a steel spoon into the bath and analyse the carbon (about 15 minutes); cut the coke so the metal stays below 0.1 % carbon.
Zana zinazohitajika:
Kokoo ya kutengeneza chuma5
5
Strip the slag and tap
Strip the slag and tap
Add 200 lb ferrosilicon and 560 lb lime to strip the slag. Tip the furnace into a preheated 5000 lb ladle: the first ladle is mostly slag, the second mostly metal. Back-pour the slag into slag pots.
Zana zinazohitajika:
Chokaa hai
Upawa wa kusubu chuma6
6
Shot the metal
Shot the metal
Pour the metal from the ladle into a second unlined 5000 lb ladle filled with running water from a 2 1/4 in fire hose, about 3000 lb a minute, from about 4 ft up; 2000 lb shots in 10 to 15 minutes. Dry the shot overnight at about 300 °F in 40 gallon drums. Ours: a drying oven.
Zana zinazohitajika:
Upawa wa kusubu chuma
Maji
Tanuri la kukaushiaVifaa
2- 1488 paundiKishikilia Nafasi
- 5000 paundiKishikilia Nafasi
Zana Zinazohitajika
11- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
Mchoro huu unatengeneza
Blueprint zinazohusiana
Blueprint hizi zinashiriki maarifa — mbinu, vifaa au kanuni
CC0 Umma Wote
Mchoro huu umetolewa chini ya CC0. Uko huru kunakili, kubadilisha, kusambaza, na kutumia kazi hii kwa madhumuni yoyote, bila kuomba ruhusa.
Saidia Mtengenezaji kwa kununua bidhaa kupitia Mchoro wao ambapo wanapata Kamisheni ya Mtengenezaji iliyowekwa na Wachuuzi, au unda marudio mapya ya Mchoro huu na uiunganishe kama kiungo katika Mchoro wako kuchangia mapato.