A paint for putting silver electrodes on ceramic, glass or mica. Silver oxide and a little ceramic flux are held in purified dextrin dissolved in water. The wet paint conducts electricity, so a capacitor can be measured while it is being painted. On firing, the silver oxide turns into a silver film held on by the flux. Dextrin needs no alcohol against foam, and silver nitrate does not attack it while the paint is in use. Source: Robert B. Gray, US 2,695,275 (Erie Resistor, 1954), Example 3. Unknown: how the dextrin is purified. Gray does not give it. Also not given: which flux, and the firing heat. Bismuth subnitrate, one of the fluxes Gray names, is ours. Picture drawn by Youblob.
Mwanzo
1 day

Maagizo

1

Dissolve 4 g purified dextrin in the water

For 100 g of paint: dissolve 4 g purified dextrin in the water. The water is the balance, about 31 to 44 g. Unknown: how the dextrin is purified. Gray does not give it.

Vifaa kwa hatua hii:

Dekstrini iliyosafishwaDekstrini iliyosafishwa4 g
Maji yaliyosafishwa kwa mvukeMaji yaliyosafishwa kwa mvuke1 as required

Zana zinazohitajika:

Mizani ya mizani-mbiliMizani ya mizani-mbili
Bikari ya BorosilikatiBikari ya Borosilikati
Fimbo ya Kioo cha BorosilikatiFimbo ya Kioo cha Borosilikati
2

Grind in silver oxide and flux

Grind 50 g precipitated silver oxide and 2 to 10 g ceramic flux into the solution until smooth. Gray gives the flux only as a class; ours: bismuth subnitrate, one of the common fluxes he names. The right amount depends on the ceramic it will be fired onto.

Vifaa kwa hatua hii:

Oksidi ya fedhaOksidi ya fedha50 g
Bismuthi subnitratiBismuthi subnitrati1 as required

Zana zinazohitajika:

Mizani ya mizani-mbiliMizani ya mizani-mbili
Kinu na mchiKinu na mchi
Glavu za NaitriliGlavu za Naitrili
3

Stir in up to 5 g silver nitrate

Stir in 0 to 5 g silver nitrate; it makes the wet paint conduct better. Dextrin is not attacked by it in normal use, and the paint can stand for hours without stirring. Silver nitrate stains and burns skin: gloves.

Vifaa kwa hatua hii:

Nitrati ya FedhaNitrati ya Fedha1 as required

Zana zinazohitajika:

Mizani ya mizani-mbiliMizani ya mizani-mbili
Fimbo ya Kioo cha BorosilikatiFimbo ya Kioo cha Borosilikati
Glavu za NaitriliGlavu za Naitrili

Vifaa

5

Zana Zinazohitajika

5

CC0 Umma Wote

Mchoro huu umetolewa chini ya CC0. Uko huru kunakili, kubadilisha, kusambaza, na kutumia kazi hii kwa madhumuni yoyote, bila kuomba ruhusa.

Saidia Mtengenezaji kwa kununua bidhaa kupitia Mchoro wao ambapo wanapata Kamisheni ya Mtengenezaji iliyowekwa na Wachuuzi, au unda marudio mapya ya Mchoro huu na uiunganishe kama kiungo katika Mchoro wako kuchangia mapato.

Majadiliano

(0)

Ingia kujiunga na majadiliano

Inapakia maoni...