Fired Silver Paint: Silver Oxide Paint with Silver Nitrate Added Just Before Use (Gray, Erie Resistor 1954, Ex. 5)
Ed

Imeundwa na

Ed

28. Oktoba 2026FI
6
0
0
0
0

Fired Silver Paint: Silver Oxide Paint with Silver Nitrate Added Just Before Use (Gray, Erie Resistor 1954, Ex. 5)

A paint for putting silver electrodes on ceramic, glass or mica. Silver oxide and a little ceramic flux are held in polyvinyl alcohol dissolved in water. The wet paint conducts electricity, so a capacitor can be measured while it is being painted. On firing, the silver oxide turns into a silver film held on by the flux. This version adds up to 3 % silver nitrate just before use, which makes the wet paint conduct better. Source: Robert B. Gray, US 2,695,275 (Erie Resistor, 1954), Example 5. Not given: which flux, and the firing heat. Bismuth subnitrate, one of the fluxes Gray names, is ours. Picture drawn by Youblob.
Mwanzo
1 day

Maagizo

1

Dissolve 2 g polyvinyl alcohol in the water

For 100 g of paint: dissolve 2 g polyvinyl alcohol in the water, warming it to help it dissolve. The water is the balance, about 34 to 44 g. Warming is ours.

Vifaa kwa hatua hii:

Unga wa polivinili alkoholiUnga wa polivinili alkoholi2 g
Maji yaliyosafishwa kwa mvukeMaji yaliyosafishwa kwa mvuke1 as required

Zana zinazohitajika:

Mizani ya mizani-mbiliMizani ya mizani-mbili
Bikari ya BorosilikatiBikari ya Borosilikati
Sahani ya Kupasha JotoSahani ya Kupasha Joto
Fimbo ya Kioo cha BorosilikatiFimbo ya Kioo cha Borosilikati
2

Grind in silver oxide and flux

Grind 50 g precipitated silver oxide and 2 to 10 g ceramic flux into the solution until smooth. Gray gives the flux only as a class; ours: bismuth subnitrate, one of the common fluxes he names. The right amount depends on the ceramic it will be fired onto.

Vifaa kwa hatua hii:

Oksidi ya fedhaOksidi ya fedha50 g
Bismuthi subnitratiBismuthi subnitrati1 as required

Zana zinazohitajika:

Mizani ya mizani-mbiliMizani ya mizani-mbili
Kinu na mchiKinu na mchi
Glavu za NaitriliGlavu za Naitrili
3

Add 2 to 4 g alcohol against foam

Stir in 2 to 4 g ethyl alcohol. It stops the polyvinyl alcohol from foaming.

Vifaa kwa hatua hii:

Etanoli ya maabara, 95 %Etanoli ya maabara, 95 %1 as required

Zana zinazohitajika:

Fimbo ya Kioo cha BorosilikatiFimbo ya Kioo cha Borosilikati
4

Add up to 3 g silver nitrate just before use

Just before painting, stir in 0 to 3 g silver nitrate. With polyvinyl alcohol it must go in immediately before use, or it breaks the binder down. Silver nitrate stains and burns skin: gloves.

Vifaa kwa hatua hii:

Nitrati ya FedhaNitrati ya Fedha1 as required

Zana zinazohitajika:

Mizani ya mizani-mbiliMizani ya mizani-mbili
Fimbo ya Kioo cha BorosilikatiFimbo ya Kioo cha Borosilikati
Glavu za NaitriliGlavu za Naitrili

Vifaa

6

Zana Zinazohitajika

6

CC0 Umma Wote

Mchoro huu umetolewa chini ya CC0. Uko huru kunakili, kubadilisha, kusambaza, na kutumia kazi hii kwa madhumuni yoyote, bila kuomba ruhusa.

Saidia Mtengenezaji kwa kununua bidhaa kupitia Mchoro wao ambapo wanapata Kamisheni ya Mtengenezaji iliyowekwa na Wachuuzi, au unda marudio mapya ya Mchoro huu na uiunganishe kama kiungo katika Mchoro wako kuchangia mapato.

Majadiliano

(0)

Ingia kujiunga na majadiliano

Inapakia maoni...