Nylon 66 Pellets: Nylon Salt Polymerised in an Autoclave, Carothers 1938
Mary

Imeundwa na

Mary

17. Oktoba 2026FI
9
0
0
0
0

Nylon 66 Pellets: Nylon Salt Polymerised in an Autoclave, Carothers 1938

Nylon salt heated to 288 °C under oxygen-free nitrogen gives off water and joins into long chains of nylon 66 (Carothers, du Pont, US 2,130,948, 1938: two moles of salt in a silver-lined autoclave). A pinch of extra adipic acid keeps the melt's viscosity steady. The polymer is then extruded and cut into pellets. The picture: our drawing of the autoclave and the pellet line.
Juu
A day

Maagizo

1

Charge the autoclave

Put two moles of nylon salt (525 g) and 0.02 mole of adipic acid (2.9 g) in a two-litre silver-lined autoclave with a stainless stirrer and a reflux condenser leading to a receiver.

Vifaa kwa hatua hii:

Chumvi ya nailoniChumvi ya nailoni525 g
Asidi ya adipikiAsidi ya adipiki2.9 g

Zana zinazohitajika:

Riakta ya shinikizoRiakta ya shinikizo
Koili ya kifidishajiKoili ya kifidishaji
Mizani ya dijitali ya jikoniMizani ya dijitali ya jikoni
2

Drive out the air

Evacuate, fill with nitrogen, evacuate again, then apply 80 lb/in² of nitrogen. Use nitrogen free of oxygen; oxygen spoils the polymer.

Zana zinazohitajika:

Pampu ya utupuPampu ya utupu
NaitrojeniNaitrojeni
Kipima ShinikizoKipima Shinikizo
3

Heat to 288 °C

Start the stirrer and heat to 288 °C over 1.5 hours.

Zana zinazohitajika:

Riakta ya shinikizoRiakta ya shinikizo
Themokapo yenye kionyeshiThemokapo yenye kionyeshi
4

Let the water off

Bring the pressure down to atmospheric over half an hour and keep heating and stirring 2.5 hours. Then pull to 200 mm absolute for a few minutes.

Zana zinazohitajika:

Riakta ya shinikizoRiakta ya shinikizo
Pampu ya utupuPampu ya utupu
Kipima ShinikizoKipima Shinikizo
Themokapo yenye kionyeshiThemokapo yenye kionyeshi
5

Cool and take out

Cool. The polymer comes out as a white solid cake that melts at about 263 °C.

Zana zinazohitajika:

Riakta ya shinikizoRiakta ya shinikizo
6

Pelletise

Break up the cake (our step), melt it in the extruder, draw the strand and cut it into pellets.

Zana zinazohitajika:

Kitoaji cha plastikiKitoaji cha plastiki
Kalibu ya kitoajiKalibu ya kitoaji
7

Grams and pressures

Inapakia daftari la Jupyter…

Vifaa

2

Zana Zinazohitajika

9

CC0 Umma Wote

Mchoro huu umetolewa chini ya CC0. Uko huru kunakili, kubadilisha, kusambaza, na kutumia kazi hii kwa madhumuni yoyote, bila kuomba ruhusa.

Saidia Mtengenezaji kwa kununua bidhaa kupitia Mchoro wao ambapo wanapata Kamisheni ya Mtengenezaji iliyowekwa na Wachuuzi, au unda marudio mapya ya Mchoro huu na uiunganishe kama kiungo katika Mchoro wako kuchangia mapato.

Majadiliano

(0)

Ingia kujiunga na majadiliano

Inapakia maoni...