Barium Ferrite Disc Magnet: Example 7 Without the Orienting Field (Gorter, Philips 1956, Ex. 7 Comparison)
Charlie

Imeundwa na

Charlie

28. Oktoba 2026DE
5
0
0
0
0

Barium Ferrite Disc Magnet: Example 7 Without the Orienting Field (Gorter, Philips 1956, Ex. 7 Comparison)

Made as in Example 7 but without the first, orienting field. Gorter's comparison blocks held 2,250 gauss with a coercive force of 1,850 oersted and a (BH)max of 0.95 × 10⁶. Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 7. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Juu
3 days

Maagizo

1

Weigh barium carbonate and iron oxide

Weigh 450 g barium carbonate and 2000 g ferric oxide. Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Vifaa kwa hatua hii:

Kabonati ya bariamu (witherite)Kabonati ya bariamu (witherite)450 g
Oksidi ya feriOksidi ya feri2000 g

Zana zinazohitajika:

Mizani ya mizani-mbiliMizani ya mizani-mbili
Glavu za mpiraGlavu za mpira
Kinga ya Kupumua ya P100Kinga ya Kupumua ya P100
2

Mill 20 hours under alcohol, dry

Grind the mixture in a ball mill under alcohol for 20 hours, then dry it.

Zana zinazohitajika:

Kinu cha mipira ya chumaKinu cha mipira ya chuma
Etanoli ya maabara, 95 %Etanoli ya maabara, 95 %
Tanuri la kukaushiaTanuri la kukaushia
3

Pre-fire: through a 1100 °C zone in 10 minutes

Pass the dry powder at 20 mm per minute through an electric furnace with a 20 cm hot zone at 1100 °C, in air: 10 minutes in the heat. Let it cool.

Zana zinazohitajika:

Tanuru ya MrijaTanuru ya Mrija
Kikaango cha kuyeyushia chenye mfuniko (kaure)Kikaango cha kuyeyushia chenye mfuniko (kaure)
Glavu Zinazostahimili JotoGlavu Zinazostahimili Joto
4

Grind 48 hours with alcohol, dry

Pulverise the pre-fired material in a ball mill with alcohol for 48 hours, then dry it. This is the pre-fired powder.

Zana zinazohitajika:

Kinu cha mipira ya chumaKinu cha mipira ya chuma
Etanoli ya maabara, 95 %Etanoli ya maabara, 95 %
Tanuri la kukaushiaTanuri la kukaushia
5

Stir into 8 % polyvinyl acetate in acetone

Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 1 cc of solution per gram of powder. The binder burns off later.

Zana zinazohitajika:

Polivinili asetatiPolivinili asetati
AsetoniAsetoni
Mizani ya mizani-mbiliMizani ya mizani-mbili
6

Mould without a first field

Put the suspension in a moulding die and remove the binder solution without any magnetic field. This is the patent's comparison block.

Zana zinazohitajika:

Kalibu ya kubana diskiKalibu ya kubana diski
Mashine ya kubana ya haidrolikiMashine ya kubana ya haidroliki
7

Heat to 500 °C in a 2000 oersted field

Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.

Zana zinazohitajika:

Tanuru ya MrijaTanuru ya Mrija
Sumaku ya umemeSumaku ya umeme
Glavu Zinazostahimili JotoGlavu Zinazostahimili Joto
8

Sinter: through a 1280 °C zone in 5 minutes

Pass the block at 20 mm per minute through an electric furnace in air at 1280 °C with a 10 cm hot zone: about 5 minutes in the heat.

Zana zinazohitajika:

Tanuru ya MrijaTanuru ya Mrija
Glavu Zinazostahimili JotoGlavu Zinazostahimili Joto
9

Magnetise the block

Magnetise the block in a field. Without the orienting field it has no preferred direction. Ours: an electromagnet. Find the north face with a compass.

Zana zinazohitajika:

Sumaku ya umemeSumaku ya umeme
DiraDira

Vifaa

2

Zana Zinazohitajika

15

Blueprint zinazohusiana

Blueprint hizi zinashiriki maarifa — mbinu, vifaa au kanuni

CC0 Umma Wote

Mchoro huu umetolewa chini ya CC0. Uko huru kunakili, kubadilisha, kusambaza, na kutumia kazi hii kwa madhumuni yoyote, bila kuomba ruhusa.

Saidia Mtengenezaji kwa kununua bidhaa kupitia Mchoro wao ambapo wanapata Kamisheni ya Mtengenezaji iliyowekwa na Wachuuzi, au unda marudio mapya ya Mchoro huu na uiunganishe kama kiungo katika Mchoro wako kuchangia mapato.

Majadiliano

(0)

Ingia kujiunga na majadiliano

Inapakia maoni...