Oriented Strontium Ferrite Disc Magnet: Agate-Milled, 10,000 Oersted Field (Gorter, Philips 1956, Ex. 8)
A strontium ferrite magnet oriented in a magnetic field: strontium carbonate and iron oxide milled, pre-fired 2 hours at 1000 °C, ground fine in an agate mill, then oriented, heated and sintered as in Example 4. In the principal direction it held 2,640 gauss with a coercive force of 2,825 oersted and a (BH)max of 1.63 × 10⁶.
Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 8. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Juu
3 days
Maagizo
1
1
Weigh strontium carbonate and iron oxide
Weigh strontium carbonate and iron oxide
Weigh 29.5 g strontium carbonate and 179 g ferric oxide.
Vifaa kwa hatua hii:
Kaboneti ya strontiamu29.5 g
Oksidi ya feri179 gZana zinazohitajika:
Mizani ya mizani-mbili
Kinga ya Kupumua ya P1002
2
Mill 15 hours with alcohol, dry
Mill 15 hours with alcohol, dry
Grind in a ball mill with alcohol for 15 hours. Remove the alcohol and dry the powder.
Zana zinazohitajika:
Kinu cha mipira ya chuma
Etanoli ya maabara, 95 %
Tanuri la kukaushia3
3
Pre-fire 2 hours at 1000 °C in air
Pre-fire 2 hours at 1000 °C in air
Heat the powder for 2 hours at 1000 °C in an electric furnace in air. Let it cool.
Zana zinazohitajika:
Tanuri ya muffle
Kikaango cha kuyeyushia chenye mfuniko (kaure)
Koleo la kaure ya kuyeyushia
Glavu Zinazostahimili Joto4
4
Grind 4 hours in an agate centrifugal mill
Grind 4 hours in an agate centrifugal mill
Grind the cooled material for 4 hours with alcohol in an agate centrifugal mill, then dry it. This is the pre-fired powder.
Zana zinazohitajika:
Kinu cha kuzunguka cha akiki
Etanoli ya maabara, 95 %
Tanuri la kukaushia5
5
Stir into 8 % polyvinyl acetate in acetone
Stir into 8 % polyvinyl acetate in acetone
Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 1 cc of solution per gram of powder. The binder burns off later.
Zana zinazohitajika:
Polivinili asetati
Asetoni
Mizani ya mizani-mbili6
6
Orient in a 10000 oersted field
Orient in a 10000 oersted field
Put the suspension in a moulding die between the poles of a magnet and apply a first field of 10000 oersted. Remove the binder solution while the field is on.
Zana zinazohitajika:
Kalibu ya kubana diski
Sumaku ya umeme
Mashine ya kubana ya haidroliki7
7
Heat to 500 °C in a 2000 oersted field
Heat to 500 °C in a 2000 oersted field
Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.
Zana zinazohitajika:
Tanuru ya Mrija
Sumaku ya umeme
Glavu Zinazostahimili Joto8
8
Sinter: through a 1280 °C zone in 5 minutes
Sinter: through a 1280 °C zone in 5 minutes
Pass the block at 20 mm per minute through an electric furnace in air at 1280 °C with a 10 cm hot zone: about 5 minutes in the heat.
Zana zinazohitajika:
Tanuru ya Mrija
Glavu Zinazostahimili Joto9
9
Magnetise in the principal direction
Magnetise in the principal direction
Magnetise the block along the direction of the first field, the principal direction. The patent magnetises it in a field in that direction; ours: an electromagnet. Find the north face with a compass.
Zana zinazohitajika:
Sumaku ya umeme
DiraVifaa
2- 29.5 gKishikilia Nafasi
- 179 gKishikilia Nafasi
Zana Zinazohitajika
17- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
Mchoro huu unatengeneza
Blueprint zinazohusiana
Blueprint hizi zinashiriki maarifa — mbinu, vifaa au kanuni
CC0 Umma Wote
Mchoro huu umetolewa chini ya CC0. Uko huru kunakili, kubadilisha, kusambaza, na kutumia kazi hii kwa madhumuni yoyote, bila kuomba ruhusa.
Saidia Mtengenezaji kwa kununua bidhaa kupitia Mchoro wao ambapo wanapata Kamisheni ya Mtengenezaji iliyowekwa na Wachuuzi, au unda marudio mapya ya Mchoro huu na uiunganishe kama kiungo katika Mchoro wako kuchangia mapato.