Strontium Ferrite Disc Magnet: Example 9 Without the Orienting Field (Gorter, Philips 1956, Ex. 9 Comparison)
Made as in Example 9 but without the first, orienting field. Gorter's comparison blocks held 2,075 gauss with a coercive force of 3,225 oersted and a (BH)max of 0.88 × 10⁶.
Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 9. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Juu
3 days
Maagizo
1
1
Weigh strontium carbonate and iron oxide
Weigh strontium carbonate and iron oxide
Weigh 29.5 g strontium carbonate and 163 g ferric oxide.
Vifaa kwa hatua hii:
Kaboneti ya strontiamu29.5 g
Oksidi ya feri163 gZana zinazohitajika:
Mizani ya mizani-mbili
Kinga ya Kupumua ya P1002
2
Mill 15 hours with alcohol, dry
Mill 15 hours with alcohol, dry
Grind in a ball mill with alcohol for 15 hours. Remove the alcohol and dry the powder.
Zana zinazohitajika:
Kinu cha mipira ya chuma
Etanoli ya maabara, 95 %
Tanuri la kukaushia3
3
Pre-fire 2 hours at 1000 °C in air
Pre-fire 2 hours at 1000 °C in air
Heat the powder for 2 hours at 1000 °C in an electric furnace in air. Let it cool.
Zana zinazohitajika:
Tanuri ya muffle
Kikaango cha kuyeyushia chenye mfuniko (kaure)
Koleo la kaure ya kuyeyushia
Glavu Zinazostahimili Joto4
4
Grind 4 hours in an agate centrifugal mill
Grind 4 hours in an agate centrifugal mill
Grind the cooled material for 4 hours with alcohol in an agate centrifugal mill, then dry it. This is the pre-fired powder. Example 9 does not say how its powder was pre-fired; ours: as in Example 8.
Zana zinazohitajika:
Kinu cha kuzunguka cha akiki
Etanoli ya maabara, 95 %
Tanuri la kukaushia5
5
Stir into 8 % polyvinyl acetate in acetone
Stir into 8 % polyvinyl acetate in acetone
Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 1 cc of solution per gram of powder. The binder burns off later.
Zana zinazohitajika:
Polivinili asetati
Asetoni
Mizani ya mizani-mbili6
6
Mould without a first field
Mould without a first field
Put the suspension in a moulding die and remove the binder solution without any magnetic field. This is the patent's comparison block.
Zana zinazohitajika:
Kalibu ya kubana diski
Mashine ya kubana ya haidroliki7
7
Heat to 500 °C in a 2000 oersted field
Heat to 500 °C in a 2000 oersted field
Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.
Zana zinazohitajika:
Tanuru ya Mrija
Sumaku ya umeme
Glavu Zinazostahimili Joto8
8
Sinter: through a 1280 °C zone in 5 minutes
Sinter: through a 1280 °C zone in 5 minutes
Pass the block at 20 mm per minute through an electric furnace in air at 1280 °C with a 10 cm hot zone: about 5 minutes in the heat.
Zana zinazohitajika:
Tanuru ya Mrija
Glavu Zinazostahimili Joto9
9
Magnetise the block
Magnetise the block
Magnetise the block in a field. Without the orienting field it has no preferred direction. Ours: an electromagnet. Find the north face with a compass.
Zana zinazohitajika:
Sumaku ya umeme
DiraVifaa
2- 29.5 gKishikilia Nafasi
- 163 gKishikilia Nafasi
Zana Zinazohitajika
17- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
Mchoro huu unatengeneza
Blueprint zinazohusiana
Blueprint hizi zinashiriki maarifa — mbinu, vifaa au kanuni
CC0 Umma Wote
Mchoro huu umetolewa chini ya CC0. Uko huru kunakili, kubadilisha, kusambaza, na kutumia kazi hii kwa madhumuni yoyote, bila kuomba ruhusa.
Saidia Mtengenezaji kwa kununua bidhaa kupitia Mchoro wao ambapo wanapata Kamisheni ya Mtengenezaji iliyowekwa na Wachuuzi, au unda marudio mapya ya Mchoro huu na uiunganishe kama kiungo katika Mchoro wako kuchangia mapato.