Polypropylene Felt: a Spunbonded Web, Kinney 1967
Tex

Imeundwa na

Tex

18. Oktoba 2026FO
7
0
0
0
0

Polypropylene Felt: a Spunbonded Web, Kinney 1967

A polypropylene felt made without weaving or needling: hot filaments are spun, pulled down by an air jet, given an electric charge so they spread apart, and laid in loops on a moving table until they form an even sheet. Kinney's patent (Du Pont, US 3,338,992, 1967) gives every setting for polypropylene. The corona runs at 20 to 25 kV: keep clear of it while it is live. The picture: the patent's own Fig. 1 (the process) and Fig. 7 (the web).
Juu
1 day

Maagizo

1

Melt and spin

Melt polypropylene of melt index 10 in a screw extruder, no hotter than 290 °C. Meter it at 12 g a minute through a 1/4 in. sand filter and a 20-hole spinneret (holes 0.015 in. across): pack block 275 °C, spinneret 260 °C.

Vifaa kwa hatua hii:

Chembechembe za polipropiliniChembechembe za polipropilini500 g

Zana zinazohitajika:

Kitoaji cha plastikiKitoaji cha plastiki
Bamba la kusokota nyuziBamba la kusokota nyuzi
Kipima joto kaliKipima joto kali
Mizani ya mizani-mbiliMizani ya mizani-mbili
Glavu za NgoziGlavu za Ngozi
2

Quench

Cool the bundle of filaments in a 6 in. quench chimney blowing 40 cubic feet a minute of room air in from the side.

Zana zinazohitajika:

Kibana hewaKibana hewa
3

Draw with the air jet

Lead the bundle 72 in. down into an air draw jet run at 25 psi: it pulls the filaments with about 3 g of tension and stretches them.

Zana zinazohitajika:

Pua ya Kuvuta kwa HewaPua ya Kuvuta kwa Hewa
Kibana hewaKibana hewa
Kipima ShinikizoKipima Shinikizo
4

Charge the filaments

8 in. above the jet, let the filaments brush a 1 1/4 in. bar turning at 10 rpm, with a four-point corona 5/8 in. from it at minus 20 to 25 kV (100 to 150 µA). The charge pushes them apart. Keep clear while it is live.

Zana zinazohitajika:

Kifaa cha kuchaji kwa koronaKifaa cha kuchaji kwa korona
5

Lay the web

Catch the filaments on a grounded 47 in. square table that moves 26 in. a minute one way and 570 in. a minute the other. Each layer weighs 0.5 oz per square yard; lay several for each sheet.

Zana zinazohitajika:

Meza ya KuwekeaMeza ya Kuwekea
6

What you get

An even sheet of fine filaments, about 2.5 denier each, tenacity 2.0 g per denier, stretching 300 % before they break.

Zana zinazohitajika:

Mizani ya mizani-mbiliMizani ya mizani-mbili

Vifaa

1

Zana Zinazohitajika

10

CC0 Umma Wote

Mchoro huu umetolewa chini ya CC0. Uko huru kunakili, kubadilisha, kusambaza, na kutumia kazi hii kwa madhumuni yoyote, bila kuomba ruhusa.

Saidia Mtengenezaji kwa kununua bidhaa kupitia Mchoro wao ambapo wanapata Kamisheni ya Mtengenezaji iliyowekwa na Wachuuzi, au unda marudio mapya ya Mchoro huu na uiunganishe kama kiungo katika Mchoro wako kuchangia mapato.

Majadiliano

(0)

Ingia kujiunga na majadiliano

Inapakia maoni...