Precipitated Silver: Silver Chloride Reduced by Zinc in Acidulated Water (Thorpe 1913)
Charlie

Imeundwa na

Charlie

28. Oktoba 2026DE
6
0
0
0
0

Precipitated Silver: Silver Chloride Reduced by Zinc in Acidulated Water (Thorpe 1913)

Fine silver powder without melting anything. Hydrochloric acid throws silver out of solution as white silver chloride. Zinc in slightly acid water then takes the chlorine away and leaves the silver as a grey powder. Source: Thorpe, Dictionary of Applied Chemistry, vol. 4 (1913), Silver. Thorpe gives no amounts, times or end-point. Ours: a silver nitrate solution, zinc sheet strips, hydrochloric acid of the two acids he names, and the washing and drying. Picture drawn by Youblob.
Mwanzo
1 day

Maagizo

1

Dissolve silver nitrate in water

Ours: dissolve silver nitrate in distilled water as the silver solution. Silver nitrate stains and burns skin: gloves and goggles.

Vifaa kwa hatua hii:

Nitrati ya FedhaNitrati ya Fedha1 as required
Maji yaliyosafishwa kwa mvukeMaji yaliyosafishwa kwa mvuke1 as required

Zana zinazohitajika:

Bikari ya BorosilikatiBikari ya Borosilikati
Fimbo ya Kioo cha BorosilikatiFimbo ya Kioo cha Borosilikati
Glavu za NaitriliGlavu za Naitrili
Miwani ya kinga dhidi ya kemikaliMiwani ya kinga dhidi ya kemikali
2

Throw down silver chloride with hydrochloric acid

Add hydrochloric acid to the solution. White silver chloride falls. Ours: add it while it still makes a precipitate, let it settle and pour off the liquid.

Vifaa kwa hatua hii:

Asidi hidroklorikiAsidi hidrokloriki1 as required

Zana zinazohitajika:

Bikari ya BorosilikatiBikari ya Borosilikati
Fimbo ya Kioo cha BorosilikatiFimbo ya Kioo cha Borosilikati
Glavu za NaitriliGlavu za Naitrili
Miwani ya kinga dhidi ya kemikaliMiwani ya kinga dhidi ya kemikali
3

Reduce the chloride with zinc in acid water

Cover the chloride with water made slightly acid with hydrochloric acid (Thorpe: hydrochloric or sulphuric) and put zinc in it. The zinc reduces the chloride to silver. Ours: strips of zinc sheet, left in until no white chloride is left. Time not given.

Vifaa kwa hatua hii:

Bati la zinkiBati la zinki1 as required
Asidi hidroklorikiAsidi hidrokloriki1 as required
Maji yaliyosafishwa kwa mvukeMaji yaliyosafishwa kwa mvuke1 as required

Zana zinazohitajika:

Bikari ya BorosilikatiBikari ya Borosilikati
Fimbo ya Kioo cha BorosilikatiFimbo ya Kioo cha Borosilikati
Glavu za NaitriliGlavu za Naitrili
Miwani ya kinga dhidi ya kemikaliMiwani ya kinga dhidi ya kemikali
4

Take out the zinc, wash and dry the silver

Ours: lift out what is left of the zinc, wash the grey silver powder with water until the washings are no longer acid, filter, and dry it. Keep it in a closed jar.

Zana zinazohitajika:

Maji yaliyosafishwa kwa mvukeMaji yaliyosafishwa kwa mvuke
Karatasi ya KuchujaKaratasi ya Kuchuja
Tanuri la kukaushiaTanuri la kukaushia
Chupa ya KiooChupa ya Kioo

Vifaa

4

Zana Zinazohitajika

8

CC0 Umma Wote

Mchoro huu umetolewa chini ya CC0. Uko huru kunakili, kubadilisha, kusambaza, na kutumia kazi hii kwa madhumuni yoyote, bila kuomba ruhusa.

Saidia Mtengenezaji kwa kununua bidhaa kupitia Mchoro wao ambapo wanapata Kamisheni ya Mtengenezaji iliyowekwa na Wachuuzi, au unda marudio mapya ya Mchoro huu na uiunganishe kama kiungo katika Mchoro wako kuchangia mapato.

Majadiliano

(0)

Ingia kujiunga na majadiliano

Inapakia maoni...