Silicone Rubber Compound: Dimethyl Silicone Oil Gelled with Ferric Oxide, Agens 1948
Mary

Imeundwa na

Mary

17. Oktoba 2026FI
6
0
0
0
0

Silicone Rubber Compound: Dimethyl Silicone Oil Gelled with Ferric Oxide, Agens 1948

Dimethyl silicone oil mixed with three-quarters its weight of red ferric oxide and a little aluminium chloride, heated to 130 °C, thins and then sets to a solid mass; milled on warm rubber rolls it becomes a silicone rubber compound ready to mould or extrude (Agens, General Electric, US 2,448,756, 1948). Cured, it stretches over 100 % and stays flexible at −60 °C. The picture: our drawing of the beaker, the mill and the sheet.
Juu
A day

Maagizo

1

Weigh the mix

To 400 g silicone oil add 300 g ferric oxide (75 % of the oil) and 5 g anhydrous aluminium chloride (1.25 %). Stir it smooth. Keep the chloride dry; it fumes in damp air.

Vifaa kwa hatua hii:

Mafuta ya silikoni ya dimethiliMafuta ya silikoni ya dimethili400 g
Unga laini wa rangi nyekundu ya kungarishaUnga laini wa rangi nyekundu ya kungarisha300 g

Zana zinazohitajika:

Kloridi ya alumini (isiyo na maji)Kloridi ya alumini (isiyo na maji)
Bikari ya BorosilikatiBikari ya Borosilikati
KikorogoKikorogo
Mizani ya dijitali ya jikoniMizani ya dijitali ya jikoni
Glavu za mpiraGlavu za mpira
2

Heat to 130 °C

Heat the mix to 130 °C. It first gets thinner, then thickens fast until the whole mass is solid.

Zana zinazohitajika:

Sahani ya Kupasha JotoSahani ya Kupasha Joto
KipimajotoKipimajoto
Bikari ya BorosilikatiBikari ya Borosilikati
3

Mill and sheet

Work the mass on rubber rolls at 125 °C for about half an hour and take it off as a sheet. This is the compound.

Zana zinazohitajika:

Kinu cha mpira cha roli mbiliKinu cha mpira cha roli mbili
KipimajotoKipimajoto
4

Test a piece

Agens's test: press a sheet about 1.3 mm thick between platens at 150 °C for ten minutes, then 15 minutes in an oven at 200 °C. It should stretch over twice its length.

Zana zinazohitajika:

Mkandamizo wa kufinyanga kwa kubana wenye jotoMkandamizo wa kufinyanga kwa kubana wenye joto
Tanuru la kulainisha metaliTanuru la kulainisha metali
5

The mix

Inapakia daftari la Jupyter…

Vifaa

2

Zana Zinazohitajika

10

CC0 Umma Wote

Mchoro huu umetolewa chini ya CC0. Uko huru kunakili, kubadilisha, kusambaza, na kutumia kazi hii kwa madhumuni yoyote, bila kuomba ruhusa.

Saidia Mtengenezaji kwa kununua bidhaa kupitia Mchoro wao ambapo wanapata Kamisheni ya Mtengenezaji iliyowekwa na Wachuuzi, au unda marudio mapya ya Mchoro huu na uiunganishe kama kiungo katika Mchoro wako kuchangia mapato.

Majadiliano

(0)

Ingia kujiunga na majadiliano

Inapakia maoni...