Strontium Ferrite Disc Magnet: 0.4 mol SrCO3 to 3.6 mol Iron Oxide, 1270 °C (Went, Philips 1956, Ex. 14)
Charlie

Imeundwa na

Charlie

28. Oktoba 2026DE
1
0
0
0
0

Strontium Ferrite Disc Magnet: 0.4 mol SrCO3 to 3.6 mol Iron Oxide, 1270 °C (Went, Philips 1956, Ex. 14)

A ceramic magnet with strontium in place of barium: 0.4 mol strontium carbonate to 3.6 mol iron oxide, milled 15 hours and passed through a 1270 °C furnace in 20 minutes. Went's rod held 1,290 gauss with a coercive force of 3,080 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 14. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Juu
2 days

Maagizo

1

Weigh strontium carbonate and iron oxide

Weigh 59.1 g strontium carbonate (0.4 mol) and 580.0 g ferric oxide (3.6 mol).

Vifaa kwa hatua hii:

Kaboneti ya strontiamuKaboneti ya strontiamu59.1 g
Oksidi ya feriOksidi ya feri580 g

Zana zinazohitajika:

Mizani ya mizani-mbiliMizani ya mizani-mbili
Kinga ya Kupumua ya P100Kinga ya Kupumua ya P100
2

Mill with alcohol 15 hours and dry

Grind with alcohol in a ball mill for 15 hours and dry.

Zana zinazohitajika:

Kinu cha mipira ya chumaKinu cha mipira ya chuma
Etanoli ya maabara, 95 %Etanoli ya maabara, 95 %
Tanuri la kukaushiaTanuri la kukaushia
3

Form the pieces and dry overnight

The patent extrudes rods; ours: press discs at 1.5 tonnes per cm², as in its other examples. Dry overnight.

Zana zinazohitajika:

Mashine ya kubana ya haidrolikiMashine ya kubana ya haidroliki
Kalibu ya kubana diskiKalibu ya kubana diski
Tanuri la kukaushiaTanuri la kukaushia
4

Pass through a 1270 °C zone in 20 minutes

Sinter in air at 1270 °C by passing the pieces through a 10 cm hot zone at 5 mm per minute: 20 minutes in the heat.

Zana zinazohitajika:

Tanuru ya MrijaTanuru ya Mrija
Glavu Zinazostahimili JotoGlavu Zinazostahimili Joto
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Zana zinazohitajika:

Sumaku ya umemeSumaku ya umeme
DiraDira

Vifaa

2

Zana Zinazohitajika

11

CC0 Umma Wote

Mchoro huu umetolewa chini ya CC0. Uko huru kunakili, kubadilisha, kusambaza, na kutumia kazi hii kwa madhumuni yoyote, bila kuomba ruhusa.

Saidia Mtengenezaji kwa kununua bidhaa kupitia Mchoro wao ambapo wanapata Kamisheni ya Mtengenezaji iliyowekwa na Wachuuzi, au unda marudio mapya ya Mchoro huu na uiunganishe kama kiungo katika Mchoro wako kuchangia mapato.

Majadiliano

(0)

Ingia kujiunga na majadiliano

Inapakia maoni...