Silver Solder of Silver and Red Copper With a Burnt Wine-Stone Flux (Theophilus, 12th Century)
How Theophilus soldered silver in the 12th century: an alloy of two parts pure silver and a third part red copper, rasped to filings, laid on a joint painted with a flux of burnt wine-stone (tartar) ground with water and salt, and flowed in the coals with a long gentle blast.
Kati
About half a day
Maagizo
1
1
The alloy
The alloy
Inapakia daftari la Jupyter…
2
2
Read De Diversis Artibus, Book III
Read De Diversis Artibus, Book III
"Weigh two parts of pure silver, and a third (part) of red copper, and mix and finely rasp into a clean vessel."
3
3
Make the solder
Make the solder
Weigh two parts of pure silver and a third part of red copper, melt them together, and rasp the alloy finely into a clean vessel; keep the filings in a quill.
Vifaa kwa hatua hii:
Fedha Safi1 kipande
Shaba-njekundu1 kipandeZana zinazohitajika:
Mizani ya mizani-mbili
Chombo cha Kuyeyushia
Koleo la kaure ya kuyeyushia
Fua ya mhunzi
Mivuo
Tupa ya mbao
Kalamu ya Unyoya4
4
Make the flux
Make the flux
Take wine-stone from a vessel in which good wine has stood a long time, tie pieces in a cloth and put it in the fire until no more vapour comes from it. When cool, blow off the cloth ash and grind the burnt stone in a copper vessel with a round mallet, mixing in water and salt until it is as thick as lees.
Vifaa kwa hatua hii:
Jiwe ghafi la divai (argol)1 kipande
Kitambaa cha Pamba1 kipande
Chumvi1 kipandeZana zinazohitajika:
Fua ya mhunzi
Ndoo ya Lita 20
Nyundo ya mbao5
5
Solder
Solder
With a thin piece of wood paint the flux round the joint inside and out, shake the filed solder over it with a small iron, and dry it. Paint more flux on, more thickly than before, put the work in the fire, cover it with coals and blow gently with a long breath until the solder has melted. Take it out, let it cool slightly and wash it. If the joint is not firm, do it again. Then file and scrape it smooth.
Zana zinazohitajika:
Fua ya mhunzi
Mivuo
Koleo la kaure ya kuyeyushia
Tupa (Tupa ya Mkono)6
6
Troubleshooting
Troubleshooting
Soldering troubleshooting.
Flow
Loading...
7
7
History and honest limits
History and honest limits
From Theophilus, **De Diversis Artibus**, Book III, chapter XXXI, translated by Robert Hendrie (1847) (checked on the archive.org scan essayuponvarious00hend, pp. 241-243). "A third (part)" can be read two ways; both are shown. Melting the alloy before rasping, the tools and the diagram are ours.
Vifaa
5- 1 kipandeKishikilia Nafasi
- 1 kipandeKishikilia Nafasi
- 1 kipandeKishikilia Nafasi
- 1 kipandeKishikilia Nafasi
- 1 kipandeKishikilia Nafasi
Zana Zinazohitajika
10- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
Mchoro huu unatengeneza
Blueprint zinazohusiana
Blueprint hizi zinashiriki maarifa — mbinu, vifaa au kanuni
CC0 Umma Wote
Mchoro huu umetolewa chini ya CC0. Uko huru kunakili, kubadilisha, kusambaza, na kutumia kazi hii kwa madhumuni yoyote, bila kuomba ruhusa.
Saidia Mtengenezaji kwa kununua bidhaa kupitia Mchoro wao ambapo wanapata Kamisheni ya Mtengenezaji iliyowekwa na Wachuuzi, au unda marudio mapya ya Mchoro huu na uiunganishe kama kiungo katika Mchoro wako kuchangia mapato.