Guitar Strings: Bronze Wound on Steel, Then Heat-Soaked (Stone and Falcone 1977)

A wound string is a steel core with another wire wrapped round it. Stone and Falcone believed the wrap keeps stresses from the winding and slowly unwinds as the string is played, so the tone goes dead. Their fix: after winding, heat-soak the string, at least 2 hours at 270 °F or 30 minutes at 480 °F for a bronze wrap, then let it cool. Source: W. N. Stone and A. S. Falcone (National Musical String Co.), US 4,063,674 (1977). Unknown: the winding itself (the patent calls it conventional), where phosphor bronze wire comes from, and the gauges. These are linked to unknown heads. The plain strings of the set are steel music wire; that, the oven and the nitrogen are ours. Picture drawn by Youblob.
Juu
1 day

Maagizo

1

Cut the core and plain strings

Cut steel music wire for the cores of the wound strings and for the plain strings of the set. Unknown: the gauges and lengths, and the ball ends.

Vifaa kwa hatua hii:

Waya wa Chuma wa Muziki 0.032"Waya wa Chuma wa Muziki 0.032"1 as required

Zana zinazohitajika:

Koleo la kukata waya la pembeKoleo la kukata waya la pembe
Vipimo visivyojulikanaVipimo visivyojulikana
2

Wind the bronze wrap at room temperature

Wrap phosphor bronze wire helically round each core at room temperature. The patent prefers a wrap that expands more with heat than the core. Unknown: how; the patent says only 'in a conventional manner'.

Vifaa kwa hatua hii:

Waya ya shaba-fosforasiWaya ya shaba-fosforasi1 as required

Zana zinazohitajika:

Njia isiyojulikana ya kuzungushaNjia isiyojulikana ya kuzungusha
Vipimo visivyojulikanaVipimo visivyojulikana
Miwani ya usalamaMiwani ya usalama
3

Heat-soak the wound strings

Heat the wound strings for a bronze wrap at 270-480 °F (132-249 °C): at least 2 hours at 270 °F or at least 30 minutes at 480 °F, shorter the hotter. If the wire tarnishes in hot air, do it without air, in nitrogen or carbon dioxide. The wrap's turns settle into more even spacing.

Zana zinazohitajika:

OveniOveni
Kipimajoto cha maabaraKipimajoto cha maabara
Silinda ya gesi ya naitrojeniSilinda ya gesi ya naitrojeni
4

Cool and set up the set

Let the strings cool back to room temperature. Make up the set with the plain steel strings.

Zana zinazohitajika:

Koleo la kukata waya la pembeKoleo la kukata waya la pembe

Vifaa

2

Zana Zinazohitajika

7

CC0 Umma Wote

Mchoro huu umetolewa chini ya CC0. Uko huru kunakili, kubadilisha, kusambaza, na kutumia kazi hii kwa madhumuni yoyote, bila kuomba ruhusa.