Metal Oxide Varistor: Pure Zinc Oxide at 1350 °C, Bismuth Oxide Paste Fired at 800 °C (Masuyama 1972, Ex. 4)
A varistor made the other way round: a disc of pure zinc oxide, sintered, with bismuth oxide fired into its faces from a paste instead of mixed in. Sintered at 1350 °C and fired with the paste at 800 °C, the disc measured a C-value of 90 at 1 mA and a nonlinearity exponent n of 7.3. Masuyama found that firing on the bismuth oxide paste raises n a great deal over mixing it in.
Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 4. Unknown: what the silver paint is, and how strong the epoxy solution of the paste is. The spraying is ours, after US Army Corps of Engineers EM 1110-2-3401 (1999). The 10 g batch is our arithmetic. Picture: the patent's drawing.
Juu
2 days
Maagizo
1
1
Press pure zinc oxide at 340 kg/cm²
Press pure zinc oxide at 340 kg/cm²
Press zinc oxide powder at 340 kg/cm². Example 4 gives no disc size; ours: discs 13 mm across and 2.5 mm thick in the mould of Example 1.
Vifaa kwa hatua hii:
Poda ya oksidi ya zinki1 as requiredZana zinazohitajika:
Mizani ya mizani-mbili
Mashine ya kubana ya haidroliki
Kalibu ya kubana diski
Kalipa ya Vernier2
2
Sinter 1 hour at 1350 °C and cool
Sinter 1 hour at 1350 °C and cool
Heat the pressed disc for 1 hour at 1350 °C, then let it cool to room temperature.
Zana zinazohitajika:
Tanuri ya muffle3
3
Lap both faces
Lap both faces
Lap both faces with silicon carbide abrasive. Example 4 gives no thickness.
Zana zinazohitajika:
Kalipa ya Vernier4
4
Coat with bismuth oxide paste and fire at 800 °C
Coat with bismuth oxide paste and fire at 800 °C
Coat both lapped faces with a paste of 50 % by weight bismuth oxide in a solution of epoxy resin in butyl alcohol, and fire it in air at 800 °C for 30 minutes. The bismuth oxide diffuses into the zinc oxide. Not given: how much paste, or the strength of the epoxy solution.
Vifaa kwa hatua hii:
Oksidi ya bismuthi1 as requiredZana zinazohitajika:
Utomvu wa epoksi
n-Butanol
Tanuri ya muffle5
5
Spray aluminium electrodes and attach leads
Spray aluminium electrodes and attach leads
Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint, as in Example 1. Ours, after US Army Corps of Engineers EM 1110-2-3401 (1999): wire-arc spray the aluminium from two 3.2 mm wires melted by an 18-40 V DC arc and atomised by compressed air, 15-20 cm from the disc and never at less than 45°, in at least two coats at right angles of 50-75 µm each. Unknown: the paint.
Vifaa kwa hatua hii:
Kitalu cha alumini1 as 3.2 mm spray wire
Rangi ya fedha inayopitisha umeme1 as required
Waya wa Shaba2 vipandeZana zinazohitajika:
Kalipa ya Vernier
Bunduki ya kunyunyiza kwa tao la waya
Kibanio hewa cha kiwandaVifaa
5- 1 as requiredKishikilia Nafasi
- 1 as requiredKishikilia Nafasi
- 1 as 3.2 mm spray wireKishikilia Nafasi
- 1 as requiredKishikilia Nafasi
- 2 vipandeKishikilia Nafasi
Zana Zinazohitajika
10- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
- Kishikilia Nafasi
Mchoro huu unatengeneza
Blueprint zinazohusiana
Blueprint hizi zinashiriki maarifa — mbinu, vifaa au kanuni
CC0 Umma Wote
Mchoro huu umetolewa chini ya CC0. Uko huru kunakili, kubadilisha, kusambaza, na kutumia kazi hii kwa madhumuni yoyote, bila kuomba ruhusa.
Saidia Mtengenezaji kwa kununua bidhaa kupitia Mchoro wao ambapo wanapata Kamisheni ya Mtengenezaji iliyowekwa na Wachuuzi, au unda marudio mapya ya Mchoro huu na uiunganishe kama kiungo katika Mchoro wako kuchangia mapato.