Glass Vial: a Corked Specimen Vial Closed and Flanged from Glass Tube (after Frary, 1914)
Bubbles

작성자

Bubbles

22. 11월 2026IT
16
0
0
0
0

Glass Vial: a Corked Specimen Vial Closed and Flanged from Glass Tube (after Frary, 1914)

A small glass vial with a cork, for specimens, gold flakes or samples: an 18 mm glass tube closed to a round bottom, cut to length and flanged at the mouth so a cork goes in without cracking it, then annealed. The methods are from Francis Frary's Laboratory Manual of Glass-Blowing (1914). About 14 ml.
중급
About 30 minutes a vial, plus practice

안내

1

Watch a test tube made

A tube closed to a round bottom at the torch (The Fusing Shop). A vial is the same, shorter, with a flanged mouth.
2

How much it holds

Jupyter 노트북 불러오는 중…

필요한 도구:

디지털 캘리퍼스 6인치디지털 캘리퍼스 6인치
3

Make a flanging tool

Frary's tool: a triangle of copper or brass about 1/16 in. (1.5 mm) thick on a handle; his Fig. 2 sizes are a = 1 in., b = 1 in. and a = 2 in., b = 1 in. Cut it from brass sheet and fit it in a slot sawn in a hardwood dowel (ours: he wraps the shank in asbestos paper, which we never use).

필요한 도구:

황동판황동판
단단한 나무 목심단단한 나무 목심
판금 가위판금 가위
줄 (손줄)줄 (손줄)
4

Close the end

Heat the tube near one end, turning it all the time, and draw it off in a short cone. Draw off the tail with a fine flame passing just below it, lifting the work out when the thread gets thin, so no lump is left. Blow out the little lump slightly, shrink the whole cone a little and blow gently to a round end like a test tube, with walls as thick as the tube's.

이 단계의 재료:

유리관유리관1 piece (18 mm x 1.2 mm wall, 200 mm)

필요한 도구:

탁상 유리 불기 토치탁상 유리 불기 토치
보안경보안경
내열 장갑내열 장갑
5

Anneal the bottom

Turn the flame smoky and hold the round end in it until coated with soot, then reduce the flame and cool it in the hot air above until it will not singe cotton wool. Let it cool fully.

필요한 도구:

탁상 유리 불기 토치탁상 유리 불기 토치
탈지면탈지면
내열 장갑내열 장갑
6

Cut to length

Make one scratch with the file edge 80 mm from the bottom (one stroke, no sawing), then pull the ends apart while bending very slightly to open the scratch. The end must be square.

필요한 도구:

줄 (손줄)줄 (손줄)
디지털 캘리퍼스 6인치디지털 캘리퍼스 6인치
내열 장갑내열 장갑
7

Flange the mouth

Turning the vial, heat only the last 2-3 mm of the mouth until it softens and starts to shrink. Warm the flanging tool, touch it to the wax, put it in at an angle and press on the soft edge while turning the vial quickly. Repeat if the flange is too small. Reheat the mouth to softening and anneal it as before.

이 단계의 재료:

파라핀 왁스파라핀 왁스1 g

필요한 도구:

탁상 유리 불기 토치탁상 유리 불기 토치
내열 장갑내열 장갑
보안경보안경
8

Fit the cork

Choose a tapered cork that starts into the mouth by about a third of its length. Twist it in; never force a cork into an unannealed vial.

이 단계의 재료:

코르크코르크1 piece (tapered, about 15 to 18 mm)
9

Troubleshooting

Vial problems and fixes.

Flow

Loading...
10

History and honest limits

From Francis C. Frary, Laboratory Manual of Glass-Blowing (1914): cutting (p. 7), flanging (pp. 11-12), the rounded test-tube end (Exercises 6 and 8) and annealing in the smoky flame (pp. 3-4). He used a gas blast lamp; borosilicate tube needs a hotter oxygen torch than soft glass. The picture shows a vial from the chemist Georg Bredig's laboratory (moulded, flat bottom); ours has a round blown bottom. Ours: the sizes, the cork and the wooden tool handle. Not made by us yet.

재료

3
  • 1 piece (18 mm x 1.2 mm wall, 200 mm)
    플레이스홀더
  • 플레이스홀더
  • 1 piece (tapered, about 15 to 18 mm)
    플레이스홀더

필요 도구

9

이 블루프린트로 만드는 것

관련 블루프린트

이 블루프린트들은 지식을 공유합니다 — 기술, 재료 또는 원리

CC0 퍼블릭 도메인