Barium Ferrite Disc Magnet: Barium Carbonate and Iron Oxide Sintered (Went, Philips 1956)
Charlie

작성자

Charlie

28. 10월 2026DE
9
0
0
0
0

Barium Ferrite Disc Magnet: Barium Carbonate and Iron Oxide Sintered (Went, Philips 1956)

The dark grey ceramic magnet on fridges and in loudspeakers is barium ferrite. It is made from two cheap powders: one part barium carbonate to six of iron oxide, milled, fired, milled again, pressed and sintered. No cobalt or nickel is needed. This is Example 34 of the Philips patent. Fired 4 hours at 1100 °C, its rod held 1,375 gauss with a coercive force of 3,350 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956). They pressed rods; the claim covers "a body of a desired shape", and the disc size is ours. The patent does not say how to magnetise it; our way is stated. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
고급
2 days

안내

1

Weigh one part barium carbonate to six of iron oxide

Weigh 39.5 g of barium carbonate (0.2 mol) and 191.7 g of ferric oxide, Fe2O3 (1.2 mol). Barium carbonate is poisonous if swallowed: ours, gloves and a dust respirator.

이 단계의 재료:

탄산바륨(독중석)탄산바륨(독중석)39.5 g
산화제이철산화제이철191.7 g

필요한 도구:

접시 저울접시 저울
고무장갑고무장갑
P100 방진 마스크P100 방진 마스크
2

Mill with ethanol for 4 hours

Grind the mixture with ethanol in an iron ball mill for 4 hours. Let the ethanol evaporate, then dry the powder in a drying oven.

필요한 도구:

철 볼 밀철 볼 밀
에탄올 - 실험실 등급, 95 %에탄올 - 실험실 등급, 95 %
건조 가마건조 가마
3

Presinter at 1000 °C for 4 hours

Fire the dry powder in air at 1000 °C for 4 hours (ours: in a lidded porcelain crucible in a muffle furnace). Let it cool.

필요한 도구:

머플로머플로
뚜껑 달린 도가니(자기)뚜껑 달린 도가니(자기)
도가니 집게도가니 집게
내열 장갑내열 장갑
4

Mill again for 4 hours

Grind the presintered product with ethanol in the ball mill for another 4 hours. Let the ethanol evaporate.

필요한 도구:

철 볼 밀철 볼 밀
에탄올 - 실험실 등급, 95 %에탄올 - 실험실 등급, 95 %
건조 가마건조 가마
P100 방진 마스크P100 방진 마스크
5

Press discs at 1.5 tons per cm²

Press the powder at 1.5 tons/cm². The patent pressed rods; we press discs. Ours: a die 20 mm across, so about 4.7 tonnes on the punch (our arithmetic: 1.5 × 3.14 cm²).

필요한 도구:

유압 프레스유압 프레스
원판 압축 금형원판 압축 금형
6

Sinter for 4 hours

Sinter the discs for 4 hours in oxygen or in air. The patent's results: at 1100 °C, 1,375 gauss and 3,350 oersted; at 1200 °C, 1,400 and 3,100; at 1300 °C, 1,850 and 1,780. Hotter gives a stronger but less stubborn magnet.

필요한 도구:

머플로머플로
도가니 집게도가니 집게
내열 장갑내열 장갑
7

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

필요한 도구:

전자석전자석
나침반나침반

재료

2

필요 도구

14

이 블루프린트로 만드는 것

CC0 퍼블릭 도메인

이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.

제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.

토론

(0)

로그인 하여 토론에 참여하세요

댓글 로딩 중...