Extruded Polystyrene Foam: Butylene-Blown Logs 20 Inches Across (McIntire, Dow 1948, Ex. 4)
Extruded polystyrene foam blown with a butylene gas fraction. 300 lb of polystyrene and about 130 lb of the fraction stand two days at 110 °C under 265 psi. Opened again and again, the tower let out foam logs 20 inches across and 20 feet long, weighing only 0.8 lb per cubic foot. Unknown: a source for the butylene fraction, linked to an unknown head.
Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 4. Picture: the patent's drawing.
고급
3 days
안내
1
1
Charge the tower with polystyrene
Charge the tower with polystyrene
Charge a high-pressure tower with 300 lb of granular polystyrene.
이 단계의 재료:
폴리스타이렌300 파운드필요한 도구:
가압 반응기
접시 저울
고무장갑2
2
Add the butylene fraction
Add the butylene fraction
Add about 130 lb of a cracked-oil gas fraction that is about 87 % normal butylenes, with some butanes and butadiene, under pressure. Unknown: a source for this fraction. Flammable gas: no flames, strong ventilation.
이 단계의 재료:
부틸렌 분해가스 유분130 파운드필요한 도구:
고압 가스통
가압 반응기
화학물질 비산 보안경3
3
Heat two days at 110 °C
Heat two days at 110 °C
Close the tower and heat it at 110 °C for two days. The gauge pressure stays at 265 psi.
필요한 도구:
가압 반응기
실험용 온도계4
4
Let out logs through a 3.25 inch outlet
Let out logs through a 3.25 inch outlet
Open and close the 3.25 inch outlet near the bottom again and again. Each portion swells into a foam log 20 inches across and about 20 feet long, with fine, even, closed cells, weighing 0.8 lb per cubic foot.
필요한 도구:
가압 반응기
화학물질 비산 보안경
고무장갑5
5
Saw into boards
Saw into boards
When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).
필요한 도구:
목공용 톱
고무장갑이 블루프린트로 만드는 것
관련 블루프린트
이 블루프린트들은 지식을 공유합니다 — 기술, 재료 또는 원리
CC0 퍼블릭 도메인
이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.
제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.