Glyptal Resin from Glycerin and Phthalic Anhydride: Callahan, 1914

Michael J. Callahan of General Electric patented this in 1914, US 1,108,329 (filed 1912): glycerin and phthalic anhydride heated together give a brittle, transparent, yellowish resin that dissolves in acetone and serves as a varnish. Heated afterwards at a moderate temperature for a long time it turns hard, infusible and insoluble, free of bubbles, with high dielectric strength, for insulating coils and wires. Resins of glycerol and phthalic acid like this were the original alkyds, sold under the name Glyptal.
고급
Workshop process

안내

1

Weigh out the charge

Jupyter 노트북 불러오는 중…
2

Fuse the charge

Mix two parts by weight of phthalic anhydride with one part of glycerin and heat slowly in a suitable container. At about 100 °C the two fuse to a clear liquid and a slight distillation begins.

이 단계의 재료:

무수 프탈산무수 프탈산2 parts by weight
글리세롤글리세롤1 part by weight

필요한 도구:

붕규산 비커붕규산 비커
전열판(핫플레이트)전열판(핫플레이트)
온도계온도계
유리 젓개유리 젓개
3

Hold at 185 °C until distillation stops

Raise the temperature to about 185 °C and keep it there until distillation ceases. Then go on heating at this temperature, or a little higher, about 210 °C, until the first stage of the reaction is complete.

필요한 도구:

전열판(핫플레이트)전열판(핫플레이트)
온도계온도계
4

Test samples and stop in time

Take small samples from the mass and let them cool. As soon as a sample is hard and brittle, without stickiness, stop heating and let the product cool. It sets to a brittle, transparent, somewhat yellowish mass that melts again on heating and dissolves in acetone. Do not heat further: the second stage then starts with a rapid rise in temperature, violent boiling sets in at about 275 °C, and the result is a hard, brittle mass full of cavities.

필요한 도구:

유리 젓개유리 젓개
온도계온도계
5

Dissolve it in acetone for varnish

Dissolve the resin in acetone. The solution is clear and can be used as a varnish: impregnate the fibrous covering of coils or wires with it, or paint it on, then evaporate the acetone.

이 단계의 재료:

아세톤아세톤1 as required

필요한 도구:

붕규산 비커붕규산 비커
유리 젓개유리 젓개
가는 붓가는 붓
6

Harden it slowly

Harden the coated or cast resin by heating it at a moderate temperature, preferably about 85 to 100 °C, for a time that depends on the mass: a layer about 0.2 inch thick takes about 15 to 20 hours. In some cases a higher temperature, say 135 °C, can be used. No bubbles form, and the product is hard, dense, infusible and practically insoluble in the usual solvents.

필요한 도구:

건조 가마건조 가마
온도계온도계

재료

3
  • 2 parts by weight
    플레이스홀더
  • 1 part by weight
    플레이스홀더
  • 1 as required
    플레이스홀더

필요 도구

6

이 블루프린트로 만드는 것

관련 블루프린트

이 블루프린트들은 지식을 공유합니다 — 기술, 재료 또는 원리

CC0 퍼블릭 도메인