Forged Flat Drills: Tool Steel Drawn to Blade and Square Taper Head, Tempered by Colour for the Metal to Be Drilled (Edwinson, 1886)
Forge

작성자

Forge

14. 11월 2026NO
30
0
0
0
0

Forged Flat Drills: Tool Steel Drawn to Blade and Square Taper Head, Tempered by Colour for the Metal to Be Drilled (Edwinson, 1886)

How a smith forged his own set of flat drills, from George Edwinson's series in Amateur Work (1886): 3/4 in. square tool steel drawn to a blade and shank with a square taper head, hardened in 45-50 F water and tempered by watching the colours run from a red-hot iron (pale straw for cast iron, orange yellow for wrought iron and copper, purplish yellow for wood), then ground to a notched gauge with clear corners.
고급
An hour or two per drill

안내

1

His sizes

Jupyter 노트북 불러오는 중…
2

Read Edwinson

"A good drill may be made to turn out good work even when all other parts are indifferently made."
3

Draw the blade

Cut a two-foot length of 3/4 in. (19 mm) square tool steel. Heat 3 in. to blood red in a clean fire, never hotter, and hammer only down to a dull red before reheating. Draw out the blade and shank first (fig. 61), close to shape.

이 단계의 재료:

공구강 봉공구강 봉1 개

필요한 도구:

대장간 화덕대장간 화덕
모루모루
망치망치
대장간 집게대장간 집게
4

Forge the head

Cut off the length for the head, hold the blade and shank in grooved flat-bit tongs, and forge a square taper head to fit your brace socket, sides equal, shank and blade central. Finish at a dull red, set true, cool.

필요한 도구:

열간 정열간 정
대장간 화덕대장간 화덕
모루모루
망치망치
대장간 집게대장간 집게
5

Shape and substance

Taper gradually from head to shank, keep the shank even for an inch or two, then let the blade swell out and thin toward the point (figs. 62, 63). Blade about 1/16 in. at the point and 1/8 in. at the corners for a 1/4 in. drill, up to 3/16 in. for 1/2 or 3/4 in.; a 1/4 in. drill's shank half as thick as a 1/2 in. blade. Leave blades a little full for grinding.

필요한 도구:

대장간 화덕대장간 화덕
모루모루
망치망치
6

Harden

Heat to red and plunge the drill straight down into cool water of 45-50 F (7-10 C), holding it until cold: icy water makes the edges brittle. Brighten the blade and part of the shank on a brick or grit-stone.

이 단계의 재료:

물물1 개

필요한 도구:

대장간 화덕대장간 화덕
양동이양동이
온도계온도계
숫돌숫돌
7

Temper by colour

Lay the shank across a red-hot piece of stout iron and watch the tints run toward the blade: straw, yellow, orange yellow, purplish yellow, purple, blues. For cast iron and hard brass stop when pale straw reaches the blade, dipping the blade to hold the later colours back while the shank cools in air. For wrought iron, soft steel or copper let the blade reach orange yellow. For wood only, let blade and shank reach purplish yellow and cool slowly.

이 단계의 재료:

물물1 개

필요한 도구:

대장간 화덕대장간 화덕
철판철판
양동이양동이
8

Grind to a gauge

Cut gauges from thin sheet brass with notches at the point angles (figs. 65, 66): very obtuse for cast iron and hard brass, more acute for wrought iron, tough steel and copper. Grind both edges equal with the point on the centre line, and give the corners clearance (fig. 70). Grind each blade to its finished size.

이 단계의 재료:

황동판황동판1 개

필요한 도구:

줄 (손줄)줄 (손줄)
회전 숫돌회전 숫돌
9

Troubleshooting

Drill troubleshooting.

Flow

Loading...
10

History and honest limits

From George Edwinson, "Smithing and Forging" IV, **Amateur Work, Illustrated**, vol. V (1886), pp. 348-351 and figs. 54-70 (checked on the archive.org scan amateurworkillus05lond; the scan reads 3/4 in. bar where the OCR text says 1/2). He also hardened glass and china drills in mercury: left out here (mercury is a poison). Metric figures, the brass gauge stock and the thermometer are ours.

재료

3
  • 플레이스홀더
  • 2 개
    플레이스홀더
  • 플레이스홀더

필요 도구

11
  • 플레이스홀더
  • 플레이스홀더
  • 플레이스홀더
  • 플레이스홀더
  • 플레이스홀더
  • 플레이스홀더
  • 플레이스홀더
  • 플레이스홀더
  • 플레이스홀더
  • 플레이스홀더
  • 플레이스홀더

이 블루프린트로 만드는 것

CC0 퍼블릭 도메인

이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.