Nichrome Wire: Nickel and Chromium Fused, Drawn and Annealed
Nichrome is the heating wire of toasters and irons. Albert Marsh patented it in 1906: nickel with less than 25 % chromium, drawn into wire and annealed, with about fifty times the resistance of copper and great resistance to oxidation when hot. Iron, he wrote, will not do. Elwood Haynes (1907) fused pure, carbon-free nickel and chromium in a magnesia crucible under an oxyhydrogen flame. White heat: face shield and gloves.
The picture: Marsh's patent drawing, a rheostat wound with the alloy (US 811,859).
고급
3 days
안내
1
1
Weigh 85 nickel to 15 chromium
Weigh 85 nickel to 15 chromium
Cut 85 g of nickel sheet into small pieces and weigh 15 g of chromium: Marsh's own example. Both must be pure and free of carbon.
이 단계의 재료:
니켈판85 g
크로뮴 금속15 g필요한 도구:
금속 가위
접시 저울2
2
Fuse under the oxyhydrogen flame
Fuse under the oxyhydrogen flame
Put the metals in a magnesia crucible, set it in a furnace lined with magnesia, and heat it with the oxyhydrogen blowpipe until both have melted together.
필요한 도구:
마그네시아 도가니
산화마그네슘
산수소 취관
도가니 집게
얼굴 가리개
가죽 장갑3
3
Cast a rod
Cast a rod
Pour the alloy into a narrow mould to get a rod that will start in the largest hole of the drawplate.
필요한 도구:
잉곳 주형
도가니 집게
얼굴 가리개
가죽 장갑4
4
Draw and anneal
Draw and anneal
Draw the rod down through the drawplate one hole at a time, as in the drawplate blueprint, and anneal it in the furnace whenever it gets hard. Marsh gives no annealing temperature. Stop at 0.41 mm (0.016 in).
필요한 도구:
강철 인발판
인발 집게
신선 윤활제
숯 도가니로
마이크로미터
가죽 장갑5
5
Check the resistance
Check the resistance
Measure one metre with the multimeter. Marsh's 15 % wire of this size measured about 2.3 ohms per foot, which is 7.5 ohms per metre.
필요한 도구:
멀티미터이 블루프린트로 만드는 것
CC0 퍼블릭 도메인
이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.