PTFE Film: Powder Rolled Thin, a Minute at 400 °C, Quenched (Brubaker & Hanford 1946)
Emma

작성자

Emma

27. 10월 2026SE
10
0
0
0
0

PTFE Film: Powder Rolled Thin, a Minute at 400 °C, Quenched (Brubaker & Hanford 1946)

Fed between two smooth rolls set 1–2 thousandths of an inch apart, PTFE powder comes out as a fragile film. One minute in a furnace at 400 °C and a dip in cold water turn it into a tough, flexible film. Rolling it again cold makes it stronger and clearer. Source: M. M. Brubaker and W. E. Hanford (du Pont), US 2,400,099 (1946), Example III. The furnace and quench bucket are ours. Picture drawn by Youblob.
고급
1 day

안내

1

Set the rolls 1–2 mils apart

Set a pair of smooth calender rolls to a gap of about 1 to 2 mils (0.001–0.002 in).

필요한 도구:

평활 캘린더 롤평활 캘린더 롤
마이크로미터마이크로미터
2

Roll the powder into film

Feed powdered PTFE between the rolls. The film that comes out is fragile: handle it gently.

이 단계의 재료:

PTFE 수지 분말PTFE 수지 분말1 as required

필요한 도구:

평활 캘린더 롤평활 캘린더 롤
3

One minute at 400 °C

Pass the film through a furnace at 400 °C so that each part stays in the heat for about 1 minute.

필요한 도구:

머플로머플로
표시기 달린 열전대표시기 달린 열전대
부집게부집게
4

Quench in cold water

Quench it straight into cold water. The film is now tough, flexible and even.

필요한 도구:

담금질 통담금질 통
5

Cold-roll it (optional)

Rolling the film again cold makes it stronger and clearer. The patent gives no gap for this pass.

필요한 도구:

평활 캘린더 롤평활 캘린더 롤
마이크로미터마이크로미터

재료

1

필요 도구

6

이 블루프린트로 만드는 것

CC0 퍼블릭 도메인

이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.

제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.

토론

(0)

로그인 하여 토론에 참여하세요

댓글 로딩 중...