PTFE Thread Seal Tape: Paste-Extruded, Calendered, Never Sintered
Emma

작성자

Emma

26. 10월 2026SE
12
0
0
0
0

PTFE Thread Seal Tape: Paste-Extruded, Calendered, Never Sintered

The white tape wound on pipe threads is PTFE that has never been melted. Fine PTFE powder is mixed with a lubricant, pressed into a slug, squeezed through a slit die by a ram, rolled thin between two rolls, and dried. Kept below the sintering heat (about 350 °C) it stays soft and conforms to the thread (process: US 5,415,939, 1995). The targets and tests are those of the Indian standard IS 14643 (from BS 4375): no fillers, at most 0.1 % lubricant left, usually 12 mm wide and 0.075 mm thick. The lubricant (naphtha) and the slitter are ours. The picture: Fig. 1a of the patent.
고급
1 day

안내

1

Wet the powder

Mix fine (dispersion-made) virgin PTFE powder with a lubricant that can be driven off completely. Granular PTFE will not paste-extrude. No fillers. Ours: naphtha, as required.

이 단계의 재료:

PTFE 파인 파우더PTFE 파인 파우더1 batch

필요한 도구:

나프타나프타
2

Press a preform

Compact the wet powder into a cylindrical preform in a mould with a plunger.

필요한 도구:

압축 성형 금형압축 성형 금형
유압 프레스유압 프레스
3

Ram-extrude a flat tape

Put the preform in the extrusion press. The plunger pushes it out through a slit die as a thick flat tape.

필요한 도구:

유압 압출 프레스유압 압출 프레스
4

Calender it thin

Pass the tape between two counter-rotating rolls to a thin tape, aiming at about 0.075 mm.

필요한 도구:

압연기압연기
마이크로미터마이크로미터
5

Dry off the lubricant

Dry the tape until the lubricant is gone. Keep it well below the sintering heat (about 350 °C): sintered tape is stiff and will not seal.

필요한 도구:

건조 가마건조 가마
6

Slit and spool

Slit it to width, usually 12 mm (±0.5 mm), and wind it on spools.

필요한 도구:

슬리터 리와인더슬리터 리와인더
7

Check the tape

It must look white, with no visible specks or torn edges. Measure the thickness at five points along a sample; each must be within 10 % of their mean.

필요한 도구:

마이크로미터마이크로미터
8

Test the residual lubricant

Weigh about 15 g of tape. Extract it in a Soxhlet with petroleum spirit (40-60 °C) for at least 4 h, dry it at 100 °C, then heat it at 300 °C for 6 h, cool and weigh. The loss must be 0.1 % or less.

필요한 도구:

속슬렛 추출기속슬렛 추출기
석유 에테르석유 에테르
건조 가마건조 가마
강철 도가니강철 도가니
건조 챔버 (소형)건조 챔버 (소형)
정밀 디지털 저울정밀 디지털 저울
9

Wrap a thread

Wind tape round an R 1/2 taper pipe thread with 50 % overlap, two layers deep, just tight enough to take the thread form. It must hold the form, not break, and its end must stay put.

필요한 도구:

나사식 배관 이음쇠나사식 배관 이음쇠

재료

1

필요 도구

14

CC0 퍼블릭 도메인

이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.

제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.

토론

(0)

로그인 하여 토론에 참여하세요

댓글 로딩 중...