Silicone Rubber Compound: Dimethyl Silicone Oil Gelled with Ferric Oxide, Agens 1948
Dimethyl silicone oil mixed with three-quarters its weight of red ferric oxide and a little aluminium chloride, heated to 130 °C, thins and then sets to a solid mass; milled on warm rubber rolls it becomes a silicone rubber compound ready to mould or extrude (Agens, General Electric, US 2,448,756, 1948). Cured, it stretches over 100 % and stays flexible at −60 °C.
The picture: our drawing of the beaker, the mill and the sheet.
고급
A day
안내
1
1
Weigh the mix
Weigh the mix
To 400 g silicone oil add 300 g ferric oxide (75 % of the oil) and 5 g anhydrous aluminium chloride (1.25 %). Stir it smooth. Keep the chloride dry; it fumes in damp air.
이 단계의 재료:
고운 붉은 광내기 가루300 g필요한 도구:
염화알루미늄(무수)
붕규산 비커
젓는 도구
디지털 주방 저울
고무장갑2
2
Heat to 130 °C
Heat to 130 °C
Heat the mix to 130 °C. It first gets thinner, then thickens fast until the whole mass is solid.
필요한 도구:
전열판(핫플레이트)
온도계
붕규산 비커3
3
Mill and sheet
Mill and sheet
Work the mass on rubber rolls at 125 °C for about half an hour and take it off as a sheet. This is the compound.
필요한 도구:
고무용 2롤 밀
온도계4
4
Test a piece
Test a piece
Agens's test: press a sheet about 1.3 mm thick between platens at 150 °C for ten minutes, then 15 minutes in an oven at 200 °C. It should stretch over twice its length.
필요한 도구:
가열식 압축 성형 프레스
풀림로5
5
The mix
The mix
Jupyter 노트북 불러오는 중…
재료
2- 400 g플레이스홀더
- 300 g플레이스홀더
이 블루프린트로 만드는 것
관련 블루프린트
이 블루프린트들은 지식을 공유합니다 — 기술, 재료 또는 원리
CC0 퍼블릭 도메인
이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.
제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.