Submerged Arc Welding
Martin

작성자

Martin

4. 8월 2026NO
1
0
0
0
0

Submerged Arc Welding

Kjellberg's coating protects the pool with a thin shell carried on the electrode. It works, but it limits how much current you can push: crank the amps up and the coating burns off ahead of the arc, spatter goes everywhere, and the operator is standing in front of a small sun.

Submerged arc welding takes the idea to its conclusion. Instead of coating the electrode, pour a deep blanket of granular flux over the joint and run a bare wire down into it. The arc burns underneath the powder, completely buried. There is no visible light, almost no spatter, no fume escaping, and no radiated heat — and because the flux blanket also traps the heat, far more of the energy goes into melting metal instead of warming the room.

US 2,043,960, “Electric Welding”, filed 9 October 1935 and granted 9 June 1936. Three inventors are named — Lloyd T. Jones, Harry E. Kennedy and Maynard A. Rotermund, assigned to Union Carbide and Carbon. Note the spelling: Rotermund, not Rothermund, and three men rather than the one the process is usually credited to.

The experiment below buries a heat source under granular material and measures what the blanket does to the energy — the principle, at a temperature you can put a thermometer on.

중급
45 minutes

안내

1

State the two claims you are testing

Write both down: a granular blanket blocks radiation, and a granular blanket keeps heat in the joint. They are separate claims.

필요한 도구:

Notebook and PencilNotebook and Pencil
2

Set up two identical steel coupons

Cut two matched coupons from the steel flat bar and sand both bright. They must start identical for the comparison to mean anything.

이 단계의 재료:

Mild Steel Flat BarMild Steel Flat Bar2
Sandpaper (220 Grit)Sandpaper (220 Grit)1

필요한 도구:

Steel Ruler (30cm)Steel Ruler (30cm)
Vernier CaliperVernier Caliper
3

Heat the open coupon and start timing

Heat coupon A to about 400 °C with the torch, then remove the flame and start the clock. Record temperature every 30 seconds.

이 단계의 재료:

Mild Steel Flat BarMild Steel Flat Bar1
FirebricksFirebricks2

필요한 도구:

Propane TorchPropane Torch
Infrared ThermometerInfrared Thermometer
Leather GlovesLeather Gloves
4

Heat the second coupon and bury it

Heat coupon B the same way, then immediately cover it with 30 mm of clean dry sand. Start the clock again.

이 단계의 재료:

Mild Steel Flat BarMild Steel Flat Bar1
Clean Dry SandClean Dry Sand2 kg

필요한 도구:

Propane TorchPropane Torch
Leather GlovesLeather Gloves
5

Track the buried coupon with the thermocouple

The infrared thermometer cannot see through sand. Use the thermocouple probe placed against the coupon before burying, and read every 30 seconds.

필요한 도구:

K-Type Thermocouple with MAX6675 ModuleK-Type Thermocouple with MAX6675 Module
6

Plot both cooling curves on one chart

Plot temperature against time for A and B together. The buried coupon holds heat markedly longer — that is the thermal-efficiency claim, confirmed.

이 단계의 재료:

Graph PaperGraph Paper1

필요한 도구:

Notebook and PencilNotebook and Pencil
7

Measure the radiation the blanket blocks

Point the infrared thermometer at each coupon's surface from 300 mm. The sand surface reads far cooler than the bare coupon. That is why no helmet is needed.

이 단계의 재료:

Graph PaperGraph Paper1

필요한 도구:

Infrared ThermometerInfrared Thermometer
Steel Ruler (30cm)Steel Ruler (30cm)
8

Test whether the blanket excludes air

Uncover coupon B once cold and compare its surface with coupon A's. The buried one carries much less scale — the sand kept oxygen out too.

필요한 도구:

Magnifying GlassMagnifying Glass
9

Weigh the scale loss on both

Brush both coupons and weigh. Quantify what you saw in step 8 rather than trusting the eye.

필요한 도구:

Digital Scale (0.01g)Digital Scale (0.01g)
File SetFile Set
10

Note what real flux does that sand cannot

Record the difference: welding flux melts to a slag, deoxidises the pool and can carry alloying elements. Sand is inert — it models the blanket, not the chemistry.

이 단계의 재료:

Notebook and PencilNotebook and Pencil1
11

Work out why the process must be mechanised

The operator cannot see the arc. Write down what that implies: the travel speed, wire feed and current must be set by machine, not judged by eye.

이 단계의 재료:

Graph PaperGraph Paper1

필요한 도구:

Notebook and PencilNotebook and Pencil
12

List where the geometry limits it

Loose powder falls off anything that is not roughly flat. Note the consequence: submerged arc welds flat and horizontal joints only — no overhead, no vertical.

이 단계의 재료:

Notebook and PencilNotebook and Pencil1
13

Safety awareness — the hazard you cannot see

An invisible arc is still an arc. Submerged arc welding is famous for needing no helmet, and that breeds carelessness: if the flux blanket thins or breaks — at the start of a run, at a joint edge, or when the hopper empties — the arc flashes through and the ultraviolet is as damaging as any other. Operators keep eye protection to hand precisely because the exposure is unexpected.

Hot flux looks exactly like cold flux. Fused slag and unfused powder are the same colour and sit side by side at wildly different temperatures. Recovered flux is handled with tools, and slag is chipped only behind eye protection — it detaches under tension and flies.

In this blueprint the sand is the hazard. Sand heated against a 400 °C coupon holds that heat for a long time and gives no visual warning at all. Leave it to cool fully and check with the thermometer before putting a hand near it.

필요한 도구:

Clear Safety GlassesClear Safety Glasses
Leather GlovesLeather Gloves
Infrared ThermometerInfrared Thermometer
14

History & Context

US 2,043,960, “Electric Welding”, filed 9 October 1935, granted 9 June 1936, assigned to Union Carbide and Carbon Corporation. The named inventors are Lloyd Theodore Jones, Harry Edward Kennedy and Maynard Arthur Rotermund — three men. The process is habitually credited to one, and the third name is regularly misspelled Rothermund. The document settles both points.

Slavyanov got there first, sort of. In the 1890s at Perm he covered the weld pool with a molten slag blanket, for the same reason. The 1936 patent is the industrialised, granular, machine-fed form of an idea that had been floating around since arc welding began — which is a fair description of a good many welding patents.

Why the numbers are so different. Because none of the energy escapes as light or radiated heat, submerged arc welding runs at currents that would be unusable in the open — commonly 300 to 1000 A and, on multi-wire installations, far more. Thermal efficiency approaches 90 per cent against roughly 60 to 70 for open-arc processes, and deposition rates are several times higher than manual stick welding. On thick plate it is not a little faster; it is a different order of magnitude.

Where you have seen it without knowing. Pressure vessels, shipbuilding, wind-turbine towers, structural I-beams and large-diameter pipe are almost all submerged arc welded, usually with the work rotating under a fixed head. It arrived just in time for the Second World War, where it welded ship hulls and armour plate at rates riveting could not approach.

The strange consequence. This is the only common welding process where the operator's protection is not equipment but the process itself. The arc is not shielded from the welder; the welder is shielded from the arc — by the same blanket that shields the weld.

재료

6

필요 도구

11

관련 블루프린트

이 블루프린트들은 지식을 공유합니다 — 기술, 재료 또는 원리

CC0 퍼블릭 도메인

이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.

제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.

토론

(0)

로그인 하여 토론에 참여하세요

댓글 로딩 중...