White Charcoal Pig Iron: Calcined Magnetic Ore Smelted with Charcoal in a Swedish Blast Furnace (Percy, 1864)

Sweden's bar iron began in small charcoal blast furnaces fed with roasted magnetic ore. Percy describes the Sten furnace and how the Swedes smelted: slow, with gentle blast, and with no hot blast at all for the best Dannemora iron, whose manganese-rich ore gives a white, crystalline pig made for the finery. Result: white pig iron in iron moulds, 40-60 tons a week; about half the weight of the ore comes out as iron. Source: John Percy, Metallurgy: Iron and Steel (1864), pp. 370-375. Picture: Percy's Fig. 54, the Swedish blast furnace.
전문가
continuous; tapped every 6 hours

안내

1

Calcine the ore

Break the magnetic ore into lumps no bigger than a double fist and roast it carefully in a mine-kiln heated by the waste gas of the furnace. The Swedes always calcine mountain ores, even without sulphur; any sulphur from pyrites is driven off.

이 단계의 재료:

자철석자철석1 ore

필요한 도구:

배소로배소로
2

Crush the roasted ore

Crush the calcined ore between grooved cast-iron rolls driven by an overshot water wheel, to pieces of ¼ to 1 cubic inch.

필요한 도구:

파쇄 롤파쇄 롤
물레방아물레방아
3

Prepare the furnace

Use a charcoal blast furnace of fire-brick in a sand-filled outer shell. Stamp the lower boshes and hearth from 6 parts crushed quartz to 1 part raw fire-clay by measure round a wooden block, and dry it very slowly with a wood fire. It has three water-cooled tuyeres about 2½ inches across.

필요한 도구:

용광로용광로
4

Set the blast

Blow with a water-driven blowing engine (at Sten three cylinders about 45 inches across, 45-inch stroke) at ½ to 1½ lb per square inch, more for hard charcoal. Keep the blast so slow that the furnace contents take at least 12 hours to pass through. For pig meant for bar iron the blast is warmed only to about 100 °C; the best Dannemora iron is made with cold blast.

필요한 도구:

송풍 기관송풍 기관
물레방아물레방아
5

Charge charcoal and ore

Charge 30-50 cubic feet of charcoal at a time and 7-10 cwt of ore on top, half spread round the sides and half in the middle, the most siliceous ore first. Dannemora ore needs no flux (other ores take 10-15 % limestone). It takes about 0.8 to 1 ton of charcoal per ton of iron.

이 단계의 재료:

숯숯1 0.8-1 ton per ton of iron

필요한 도구:

용광로용광로
6

Tap into iron moulds

Tap every 6 hours and run the metal into iron moulds, not sand. A furnace makes 40-60 tons a week; the cinder runs thin and holds under 1 % iron. Pig from Dannemora ore is white and crystalline, from its manganese.

필요한 도구:

잉곳 주형잉곳 주형

재료

2
  • 플레이스홀더
  • 1 0.8-1 ton per ton of iron
    플레이스홀더

필요 도구

6
  • 플레이스홀더
  • 플레이스홀더
  • 플레이스홀더
  • 플레이스홀더
  • 플레이스홀더
  • 플레이스홀더

이 블루프린트로 만드는 것

관련 블루프린트

이 블루프린트들은 지식을 공유합니다 — 기술, 재료 또는 원리

CC0 퍼블릭 도메인

이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.

제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.

토론

(0)

로그인 하여 토론에 참여하세요

댓글 로딩 중...