Guitar Strings: Bronze Wound on Steel, Then Heat-Soaked (Stone and Falcone 1977)
A wound string is a steel core with another wire wrapped round it. Stone and Falcone believed the wrap keeps stresses from the winding and slowly unwinds as the string is played, so the tone goes dead. Their fix: after winding, heat-soak the string, at least 2 hours at 270 °F or 30 minutes at 480 °F for a bronze wrap, then let it cool.
Source: W. N. Stone and A. S. Falcone (National Musical String Co.), US 4,063,674 (1977). Unknown: where phosphor bronze wire comes from, and the gauges. The winding, which the patent calls conventional, is ours, after Landtroop and Dykstra, US 6,256,872 (2001). These are linked to unknown heads. The plain strings of the set are steel music wire; that, the oven and the nitrogen are ours. Picture drawn by Youblob.
고급
1 day
안내
1
1
Cut the core and plain strings
Cut the core and plain strings
Cut steel music wire for the cores of the wound strings and for the plain strings of the set. Unknown: the gauges and lengths, and the ball ends.
이 단계의 재료:
강철 피아노선 0.032인치1 as required필요한 도구:
니퍼
알 수 없는 치수2
2
Wind the bronze wrap at room temperature
Wind the bronze wrap at room temperature
Wrap phosphor bronze wire helically round each core at room temperature. The patent prefers a wrap that expands more with heat than the core. The patent says only 'in a conventional manner'. Ours, after Landtroop and Dykstra, US 6,256,872 (2001): hook the core's ball end on the motor-driven headstock spindle, grip the other end in the tailstock chuck and stretch it with the tailstock tension cylinder; fix the end of the cover wire at the ball end, then spin the core while a carriage travels toward the tailstock, paying the cover wire out under tension from its spool; cut it off at the end.
이 단계의 재료:
인청동 와이어1 as required필요한 도구:
현 감기 기계
알 수 없는 치수
보안경3
3
Heat-soak the wound strings
Heat-soak the wound strings
Heat the wound strings for a bronze wrap at 270-480 °F (132-249 °C): at least 2 hours at 270 °F or at least 30 minutes at 480 °F, shorter the hotter. If the wire tarnishes in hot air, do it without air, in nitrogen or carbon dioxide. The wrap's turns settle into more even spacing.
필요한 도구:
오븐
실험용 온도계
질소 가스 실린더4
4
Cool and set up the set
Cool and set up the set
Let the strings cool back to room temperature. Make up the set with the plain steel strings.
필요한 도구:
니퍼이 블루프린트로 만드는 것
관련 블루프린트
이 블루프린트들은 지식을 공유합니다 — 기술, 재료 또는 원리
CC0 퍼블릭 도메인
이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.
제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.