Zinc Powder: Zinc Crushed Hot, Just Below Melting
Zinc has an odd temper: brittle cold, soft enough to roll at 100 to 150 °C, and above 200 °C so tender that it crushes to powder. Thorpe (1913): zinc dust can be made by crushing the metal in a mortar at a heat somewhat below its melting point of 420 °C. Work hot with leather gloves.
The picture: our own drawing.
초급
Half a day
안내
1
1
Cut the zinc small
Cut the zinc small
Saw 300 g of zinc into small pieces.
이 단계의 재료:
아연 잉곳300 g필요한 도구:
쇠톱(핵소)
접시 저울2
2
Heat to just below melting
Heat to just below melting
Heat the pieces in an iron pot above 200 °C but below 420 °C, where zinc melts. Check with a pyrometer.
필요한 도구:
무쇠 솥
숯 화로
고온계
가죽 장갑3
3
Crush in the mortar
Crush in the mortar
Tip a few hot pieces at a time into the mortar and crush them. Hot zinc breaks to powder; reheat what is left whole.
필요한 도구:
막자사발과 막자
가죽 장갑4
4
Sieve and store
Sieve and store
Sieve the cooled powder, return the coarse bits for another crushing, and keep the powder in a closed jar.
필요한 도구:
고운 체
뚜껑 있는 유리병이 블루프린트로 만드는 것