Swedish Bar Iron: White Pig Iron Refined in a Walloon Finery and Drawn under Water Hammers, as at Dannemora (Percy, 1864)
Forge

නිර්මාතෘ

Forge

1. නොවැම්බර් 2026NO
4
0
0
0
0

Swedish Bar Iron: White Pig Iron Refined in a Walloon Finery and Drawn under Water Hammers, as at Dannemora (Percy, 1864)

The renowned bar iron of Dannemora was refined in the old Walloon way: long white pigs melt drop by drop before a cold blast in a small, very hot charcoal hearth, the finer works the metal with an iron staff until it comes to nature, and the lump is drawn out under water-driven hammers. Result: bars 12 ft long of about 60 lb; 6 tons a week from one hearth, 80 % of the weight of the pig. Source: John Percy, Metallurgy: Iron and Steel (1864), pp. 599-601, after Tunner and A. Grill. Picture drawn by Youblob.
විශේෂඥ
about 30 minutes per lump; 8-hour shifts

උපදෙස්

1

Build the finery hearth

Make the hearth of cast-iron plates: a 2-inch bottom plate on about 3 inches of pounded slag, over a cast-iron box with channels to drain water. From the tuyere it is 10-11½ inches to the back-plate, 22-24 inches to the work-plate and 22-24 inches to the opposite side. Depth: 7-8 inches under the tuyere, 14-15 under the back-plate, 15-18 opposite the tuyere. No tapping hole: the slag is never let out.

අවශ්‍ය මෙවලම්:

පිරිපහදු උදුනපිරිපහදු උදුන
2

Set the tuyere and blast

The tuyere nozzle is semicircular, flat side down, 20-25 lines broad and 16-17 lines high, and projects 3½ inches; the blast-pipe nozzle sits 4 inches back inside it. Use cold blast. The blowing machine is not described.

අවශ්‍ය මෙවලම්:

පිරිපහදු උදුනපිරිපහදු උදුන
පිඹින බෙල්ලුමපිඹින බෙල්ලුම
3

Lay in the pigs

Use white or strongly mottled pig in long pigs about 9 inches broad, 15-18 feet long, 3-4 inches thick at one end and 1-2 at the other. Lay them across the back-plate, one end sloping down over the tuyere, usually two one above the other, and push them forward as the ends melt.

මෙම පියවර සඳහා ද්‍රව්‍ය:

සුදු අඟුරු පිග් යකඩසුදු අඟුරු පිග් යකඩ1 long pigs

අවශ්‍ය මෙවලම්:

පිරිපහදු උදුනපිරිපහදු උදුන
4

Light and make the slag bath

Fill the front of the hearth with moistened small charcoal and the rest with charcoal, light it and turn on the blast. To make enough slag bath, melt down some large finery scraps or, failing these, several shovelfuls of hammer scale.

අවශ්‍ය මෙවලම්:

දර අඟුරු - සිහින්ව අඹරන ලදදර අඟුරු - සිහින්ව අඹරන ලද
ජලයජලය
අඟුරුඅඟුරු
යකඩ කබොලයකඩ කබොල
උදැල්ල (කර)උදැල්ල (කර)
5

Reheat the last bloom

At the start of each heat, hold the bloom from the last lump with tongs, as steeply as you can, in the front of the hearth to reheat it for drawing out.

අවශ්‍ය මෙවලම්:

කම්මල්කරුගේ අඬුවකම්මල්කරුගේ අඬුව
6

Work the metal with the staff

As soon as the first pig iron melts, work it with an iron staff: bring the metal on the tuyere side up from the bottom towards the middle into the blast, once to the left and once to the right of the reheating bloom. About 70 lb melts in 20 minutes; thin pieces of malleable iron then cling to the staff.

අවශ්‍ය මෙවලම්:

වට යකඩ දණ්ඩවට යකඩ දණ්ඩ
7

Form the lump

Stop the flow of fresh molten pig, break up all the metal above the tuyere, melt it down and gather it into a lump about 12 by 15 inches. One lump takes 28 minutes on average (25-30).

අවශ්‍ය මෙවලම්:

වට යකඩ දණ්ඩවට යකඩ දණ්ඩ
කම්මල්කරුගේ අඬුවකම්මල්කරුගේ අඬුව
8

Draw out the bar

Heat each lump 6-8 times in a separate fire and draw it out under water-driven hammers into a bar 12 feet long of about 60 lb. One finery, one drawing-out forge and one hammer make 6 tons of bars a week; the bars weigh 80 % of the pig, and take 3 tons of charcoal per ton.

අවශ්‍ය මෙවලම්:

කම්මල් උදුනකම්මල් උදුන
පතන මිටියපතන මිටිය
දිය රෝදයදිය රෝදය
කම්මල්කරුගේ අඬුවකම්මල්කරුගේ අඬුව

ද්‍රව්‍ය

1

අවශ්‍ය මෙවලම්

12

මෙම සැලසුම සාදන්නේ

සම්බන්ධ බ්ලූප්‍රින්ට්

මෙම බ්ලූප්‍රින්ට් දැනුම බෙදා ගනී — ශිල්ප ක්‍රම, ද්‍රව්‍ය හෝ මූලධර්ම

CC0 පොදු වසම

මෙම බ්ලූප්‍රින්ට් CC0 යටතේ නිකුත් කර ඇත. ඔබට අවසර නොමැතිව පිටපත් කිරීම, වෙනස් කිරීම, බෙදා හැරීම සහ භාවිතා කිරීම කළ හැක.

බ්ලූප්‍රින්ට් හරහා නිෂ්පාදන මිලදී ගැනීමෙන් නිර්මාතෘට සහාය වන්න නිර්මාතෘ කොමිසම විකුණුම්කරුවන් විසින් නියම කළ, හෝ මෙම බ්ලූප්‍රින්ට්හි නව අනුවාදයක් සාදා ආදායම බෙදා ගැනීමට ඔබේ බ්ලූප්‍රින්ට්හි සම්බන්ධතාවයක් ලෙස ඇතුළත් කරන්න.

සාකච්ඡාව

(0)

පිවිසෙන්න සාකච්ඡාවට එක්වීමට

අදහස් පූරණය කරමින්...