Electrolytic Iron: Brown Ferrous Electrolyte, Rotating Cathode at 75-77 °C, Graphite Anodes (Bouchayer, US 1,516,326)

Iron plated out of a fresh green ferrous bath comes off rough and useless. Bouchayer first stirred the bath in air until it turned bright brown; the iron oxychloride formed takes care of the hydrogen at the cathode, and the deposit grows even and compact at high current. Result: electrolytic iron, deposited at about 98 % current yield. Source: Bouchayer, US 1,516,326 (1924). Not given: cathode material, purity of the iron. Picture drawn by Youblob.
Дээд шат
Factory process

Зааварчилгаа

1

Make up the electrolyte at 20 °Bé

Dissolve ferrous sulfate in water (Bouchayer also allows ferrous chloride or a mix). Concentration: e.g. 20 °Bé, then keep it constant.

Энэ алхмын материал:

Төмрийн сульфатТөмрийн сульфат1 as required

Шаардлагатай багаж:

УсУс
Нягт хэмжигчНягт хэмжигч
Электролизийн савЭлектролизийн сав
2

Stir it in air until brown

Agitate the green bath in air, e.g. by turning the anode, until it is bright brown and stops foaming. Used green, it gives only an irregular deposit.

Шаардлагатай багаж:

Электролизийн савЭлектролизийн сав
3

Circulate it through iron filings

Pump the electrolyte through a mass of iron filings in a separate vessel; it takes back iron and forms the ferric hydroxide that keeps the bath working. Keep it moving fast past the anodes: this lowers the phosphorus.

Энэ алхмын материал:

Төмрийн үртэсТөмрийн үртэс1 as required

Шаардлагатай багаж:

Усны насосУсны насос
4

Deposit on a rotating cathode

Electrolyse between graphite anodes and a rotating cathode. Temperature: e.g. 75-77 °C at 1000 A/m², held exactly constant and below boiling; cathode speed: e.g. 120 m/min at 800 A/m². Cathode material: not given.

Шаардлагатай багаж:

Бал чулууны электродБал чулууны электрод
Шууд урсгалын тэжээлийн үүсгүүрШууд урсгалын тэжээлийн үүсгүүр
ТермометрТермометр
Электролизийн савЭлектролизийн сав
5

Strip and reheat the deposit

Take the compact iron deposit off the cathode; it is usable after a slight reheating (temperature not given).

Шаардлагатай багаж:

Электролизийн савЭлектролизийн сав

Материал

2

Шаардлагатай багаж

7

Холбоотой загварууд

Эдгээр загварууд мэдлэг хуваалцдаг — арга техник, материал эсвэл зарчим

CC0 Нийтийн домэйн

Энэ загвар CC0 дор гаргагдсан. Та зөвшөөрөл авахгүйгээр хуулах, өөрчлөх, түгээх, ашиглах боломжтой.

Загвараар дамжуулан бүтээгдэхүүн худалдаж авч Бүтээгчийг дэмжээрэй Бүтээгчийн шимтгэл Борлуулагчаар тогтоосон, эсвэл энэ загварын шинэ хувилбар үүсгэж орлогоо хуваахын тулд өөрийн загварт холбоос болгон оруулна уу.

Хэлэлцүүлэг

(0)

Нэвтрэх хэлэлцүүлэгт нэгдэхийн тулд

Сэтгэгдлүүдийг ачаалж байна...