Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 60 °C (McIntire, Dow 1948, Ex. 3, Test 3)
Charlie

Зохиогч

Charlie

28. Аравдугаар сар 2026DE
11
0
0
0
0

Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 60 °C (McIntire, Dow 1948, Ex. 3, Test 3)

Extruded polystyrene foam blown with a propylene gas fraction instead of methyl chloride. Polystyrene stands two days at 40 °C with the propylene under pressure and becomes a gel. Let out at 60 °C (300 psi in the tower), it swelled into a log 11 inches across, weighing 3.08 lb per cubic foot, with small uniform cells. Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 3. Picture: the patent's drawing.
Дээд шат
3 days

Зааварчилгаа

1

Charge the tower with polystyrene

Charge a high-pressure tower with 300 lb of granular polystyrene.

Энэ алхмын материал:

ПолистиролПолистирол300 фунт

Шаардлагатай багаж:

Даралтат реакторДаралтат реактор
Дэнсний жинлүүрДэнсний жинлүүр
Резинэн бээлийРезинэн бээлий
2

Add the propylene fraction

Add 100 lb of a cracked-oil gas fraction that is about 93 % propylene, under pressure, and close the tower. Propylene is a flammable gas: no flames, strong ventilation.

Энэ алхмын материал:

ПропиленПропилен100 фунт

Шаардлагатай багаж:

Даралтат хийн баллонДаралтат хийн баллон
Даралтат реакторДаралтат реактор
Химийн цацралтын нүдний шилХимийн цацралтын нүдний шил
3

Stand two days at 40 °C

Let the tower stand for two days at 40 °C while the polystyrene takes up the propylene.

Шаардлагатай багаж:

Даралтат реакторДаралтат реактор
Лабораторийн термометрЛабораторийн термометр
4

Let it out at 60 °C

Open the valved outlet near the bottom (2.5 inch in the patent) at 60 °C. The pressure is about 300 psi. The gel flows out and swells into a log 11 inches across, 3.08 lb per cubic foot, with small uniform cells. Close the outlet again. The patent heated step by step (50, 60, 75 °C) for several hours each, letting a portion out at each step.

Шаардлагатай багаж:

Даралтат реакторДаралтат реактор
Лабораторийн термометрЛабораторийн термометр
Химийн цацралтын нүдний шилХимийн цацралтын нүдний шил
Резинэн бээлийРезинэн бээлий
5

Saw into boards

When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).

Шаардлагатай багаж:

Мужааны хөрөөМужааны хөрөө
Резинэн бээлийРезинэн бээлий

Материал

2
  • Түр орлуулагч
  • 100 фунт
    Түр орлуулагч

Шаардлагатай багаж

7

Холбоотой загварууд

Эдгээр загварууд мэдлэг хуваалцдаг — арга техник, материал эсвэл зарчим

CC0 Нийтийн домэйн

Энэ загвар CC0 дор гаргагдсан. Та зөвшөөрөл авахгүйгээр хуулах, өөрчлөх, түгээх, ашиглах боломжтой.

Загвараар дамжуулан бүтээгдэхүүн худалдаж авч Бүтээгчийг дэмжээрэй Бүтээгчийн шимтгэл Борлуулагчаар тогтоосон, эсвэл энэ загварын шинэ хувилбар үүсгэж орлогоо хуваахын тулд өөрийн загварт холбоос болгон оруулна уу.

Хэлэлцүүлэг

(0)

Нэвтрэх хэлэлцүүлэгт нэгдэхийн тулд

Сэтгэгдлүүдийг ачаалж байна...