Longquan Celadon Bowls: Glaze of Glaze Stone, Husk-and-Lime Ash and Zijin Clay, Reduction Fired
Clay

Зохиогч

Clay

1. Арван нэгдүгээр сар 2026DK
12
0
0
0
0

Longquan Celadon Bowls: Glaze of Glaze Stone, Husk-and-Lime Ash and Zijin Clay, Reduction Fired

Longquan celadon, made in Longquan, China, since the 10th century, is a thick jade-green glaze over a bisque-fired body. The glaze is three powders washed out of local materials: glaze stone, the ash of rice husk burnt together with limestone, and iron-rich Zijin clay. Fired in reduction between 900 and 1230 °C, the iron in the glaze turns blue-green. Result: thick-glazed, jade-green celadon bowls. Source: the video 'Longquan celadon' by Shanbai (2025), checked frame by frame against its captions. Not given: amounts, the glaze proportion, ageing times, how iron is taken out, firing times. Unknown: the clay body of the bowls; the video does not show it. Photo: Southern Song Longquan bowl, Royal Ontario Museum, by Daderot (CC0).
Дээд шат
several weeks

Зааварчилгаа

1

Watch: Longquan celadon from stone to bowl

The whole process in eight minutes, by Shanbai: preparing the three glaze materials, throwing and bisque firing the bowls, glazing, and the reduction firing.
2

Pound the glaze stone

Crush the glaze stone in a stone mortar with a foot-trodden pestle.

Энэ алхмын материал:

Паалангийн чулууПаалангийн чулуу1 as required

Шаардлагатай багаж:

Хөлөөр гишгэдэг нүдүүрХөлөөр гишгэдэг нүдүүр
3

Sieve and settle the stone

Sieve the crushed stone and pound the coarse bits again. Stir the fine stone into water in a vat, sieve off the fine particles suspended in the water into another vat, and let them settle.

Шаардлагатай багаж:

Шигшүүрийн багц (шатлалт нүх)Шигшүүрийн багц (шатлалт нүх)
УсУс
Таглаатай керамик савТаглаатай керамик сав
ШанагаШанага
4

Burn rice husk with limestone

In a brick-edged bed outdoors, lay rice husk and limestone in alternate layers and burn them. Turn the materials several times during the firing so the husk burns completely.

Энэ алхмын материал:

Будааны хальсБудааны хальс1 as required
Шохойн чулууны блокШохойн чулууны блок1 as required

Шаардлагатай багаж:

ТоосгоТоосго
ХүрзХүрз
5

Sieve and wash the ash

Sieve the ash into a vat. Add water and ladle it through a fine sieve into a fresh vat. While this 'black glaze' settles, change the water and wash it several times.

Шаардлагатай багаж:

Шигшүүрийн багц (шатлалт нүх)Шигшүүрийн багц (шатлалт нүх)
Таглаатай керамик савТаглаатай керамик сав
УсУс
ШанагаШанага
6

Mill and settle the Zijin clay

Grind the dry Zijin clay to powder in a stone hand mill. Mix it well with water, sieve it into a fresh vat and let the fine particles settle.

Энэ алхмын материал:

Зыцзинь шаварЗыцзинь шавар1 as required

Шаардлагатай багаж:

Чулуун гар тээрэмЧулуун гар тээрэм
УсУс
Шигшүүрийн багц (шатлалт нүх)Шигшүүрийн багц (шатлалт нүх)
Таглаатай керамик савТаглаатай керамик сав
7

Dewater in bags, then age

Drain the water off each of the three vats without stirring up the settled powder. Scoop each paste into a cloth bag, lay the bags on a board and press them under a millstone. When they are dewatered to a certain degree, let them age for a while. Not given: how long. Ours: linen bags (as in the transcript).

Шаардлагатай багаж:

ШанагаШанага
Маалингын уутМаалингын уут
Гар тээрмийн чулууГар тээрмийн чулуу
8

Throw the bowls

Throw the bowls on the wheel and let them air-dry in the shade. Unknown: the clay body; the video does not show what it is or how it is made.

Энэ алхмын материал:

Үл мэдэгдэх шаварлаг биеҮл мэдэгдэх шаварлаг бие1 as required

Шаардлагатай багаж:

Ваарчны хүрдВаарчны хүрд
9

Trim and stamp

Set each dry bowl upside down on a chuck on the wheel, trim the outside and the foot smooth, and stamp your mark in the foot.

Шаардлагатай багаж:

Ваарчны хүрдВаарчны хүрд
Түүхий мод эрэгдэх багажТүүхий мод эрэгдэх багаж
Ваарчны тамгаВаарчны тамга
10

Bisque fire at about 800 °C

Stack the bowls in the kiln, brick up the door and seal it with mud, and fire with wood to about 800 °C. The bisque firing makes the body stronger and more absorbent, so the glaze takes better.

Шаардлагатай багаж:

Шатаах зуухШатаах зуух
ТоосгоТоосго
ТүлээТүлээ
ПирометрПирометр
11

Make the glaze

Mix the burnt husk-and-lime ash, the glaze stone and the Zijin clay in proportion, add about an equal amount of water, stir and grind fine. Sieve it, take out the iron, and let the glaze age in the glaze vat. Not given: the proportion, how the iron is removed, how long it ages. Rice husk ash, glaze stone and Zijin clay give the silica, feldspar and kaolin; Zijin clay's iron is the colourant; lime and the potash and soda of feldspar lower the melting point.

Шаардлагатай багаж:

Чулуун уур ба нүдүүрЧулуун уур ба нүдүүр
УсУс
Шигшүүрийн багц (шатлалт нүх)Шигшүүрийн багц (шатлалт нүх)
Таглаатай керамик савТаглаатай керамик сав
12

Dip the bowls

Hold each bisque bowl with wire tongs and dip it into the glaze. Let it air-dry.

Шаардлагатай багаж:

Дүрэх хавчаарДүрэх хавчаар
Таглаатай керамик савТаглаатай керамик сав
13

Spray on more glaze

Set the bowl upside down on a chuck on the wheel and spray glaze evenly over the outside with a mouth-blown sprayer. Repeated bisque firings, dipping and thin spray coats build a thick glaze; Longquan celadon is a lime-alkali glaze that stays put at high temperature. Scrape the glaze off the foot with a knife.

Шаардлагатай багаж:

Ваарчны хүрдВаарчны хүрд
Амаар үлээх паалан шүршигчАмаар үлээх паалан шүршигч
ХутгаХутга
14

Reduction fire in saggars

Set the bowls in saggars, stack them in the kiln and seal the door. Between 900 °C and 1230 °C, feed fuel often, and when combustion is insufficient fire in reduction: the iron in the glaze gives up oxygen, and the mix of divalent and trivalent iron turns the glaze blue-green. Not given: how long the firing takes.

Шаардлагатай багаж:

Галд тэсвэртэй хайрцаг (саггер)Галд тэсвэртэй хайрцаг (саггер)
Шатаах зуухШатаах зуух
ТоосгоТоосго
ТүлээТүлээ
ПирометрПирометр

Материал

5

Шаардлагатай багаж

21

Холбоотой загварууд

Эдгээр загварууд мэдлэг хуваалцдаг — арга техник, материал эсвэл зарчим

CC0 Нийтийн домэйн

Энэ загвар CC0 дор гаргагдсан. Та зөвшөөрөл авахгүйгээр хуулах, өөрчлөх, түгээх, ашиглах боломжтой.

Загвараар дамжуулан бүтээгдэхүүн худалдаж авч Бүтээгчийг дэмжээрэй Бүтээгчийн шимтгэл Борлуулагчаар тогтоосон, эсвэл энэ загварын шинэ хувилбар үүсгэж орлогоо хуваахын тулд өөрийн загварт холбоос болгон оруулна уу.

Хэлэлцүүлэг

(0)

Нэвтрэх хэлэлцүүлэгт нэгдэхийн тулд

Сэтгэгдлүүдийг ачаалж байна...