Neodymium Metal: Oxide Reduced by Graphite in Vacuum, Distilled at 1900 °C onto Tantalum (Downing, Union Carbide, US 3,104,970)
Charlie

Зохиогч

Charlie

31. Аравдугаар сар 2026DE
11
0
0
0
0

Neodymium Metal: Oxide Reduced by Graphite in Vacuum, Distilled at 1900 °C onto Tantalum (Downing, Union Carbide, US 3,104,970)

Carbon cannot pull neodymium out of its oxide in an ordinary furnace. In a hard vacuum it can: the oxide and graphite turn into neodymium carbide, and at 1900 °C the neodymium itself boils off and condenses as metal on a cool tantalum plate. Result: neodymium metal, 99.21 % Nd and 0.83 % carbon in Union Carbide's run. Source: Downing, Gorski and Koerner, US 3,104,970 (Union Carbide, 1963), Example II. That example starts from a samarium-neodymium mixture; using it for pure neodymium oxide is ours. Picture drawn by Youblob.
Дээд шат
2 days

Зааварчилгаа

1

Mix with graphite and pelletise

Mix the oxide intimately with powdered graphite (Example II: 78 % oxides to 22 % graphite by weight, 1.8 % carbon over theory; the patent allows 1-15 %, prefers 5-10 %), particles under about 50 microns, and press into 0.75 in pellets.

Энэ алхмын материал:

Неодимын исэлНеодимын исэл78 parts
Бал чулууны нунтагБал чулууны нунтаг22 parts

Шаардлагатай багаж:

Дэнсний жинлүүрДэнсний жинлүүр
Шахмал прессийн машинШахмал прессийн машин
2

Reduce in vacuum to the carbide

Heat the pellets in a vacuum induction furnace at 0.15 micron for about 8 hours. The example's temperature is printed "1700-1700 °C"; claim 5 gives about 1920 °C for about 16 hours. Volatile matter goes to a graphite condenser; the neodymium stays behind as carbide.

Шаардлагатай багаж:

Индукцийн хайлуулах зуухИндукцийн хайлуулах зуух
Вакуум насосВакуум насос
Бал чулуун тигельБал чулуун тигель
3

Purge at 1600 °C

Reheat the carbide residue in a carbon crucible at 1600 °C and 0.05 micron for 1 hour (in the example this drove off the last samarium). The residue is substantially pure neodymium carbide.

Шаардлагатай багаж:

Индукцийн хайлуулах зуухИндукцийн хайлуулах зуух
Вакуум насосВакуум насос
Бал чулуун тигельБал чулуун тигель
4

Distil the metal at 1900 °C onto tantalum

Heat it in a graphite crucible to 1900 °C at 0.05 micron for 3 hours. Neodymium boils off and condenses on a tantalum plate, which barely alloys with it: 99.21 % neodymium, 0.83 % carbon.

Шаардлагатай багаж:

Индукцийн хайлуулах зуухИндукцийн хайлуулах зуух
Вакуум насосВакуум насос
Бал чулуун тигельБал чулуун тигель
Танталын конденсатор хавтанТанталын конденсатор хавтан

Материал

2

Шаардлагатай багаж

6

Холбоотой загварууд

Эдгээр загварууд мэдлэг хуваалцдаг — арга техник, материал эсвэл зарчим

CC0 Нийтийн домэйн

Энэ загвар CC0 дор гаргагдсан. Та зөвшөөрөл авахгүйгээр хуулах, өөрчлөх, түгээх, ашиглах боломжтой.

Загвараар дамжуулан бүтээгдэхүүн худалдаж авч Бүтээгчийг дэмжээрэй Бүтээгчийн шимтгэл Борлуулагчаар тогтоосон, эсвэл энэ загварын шинэ хувилбар үүсгэж орлогоо хуваахын тулд өөрийн загварт холбоос болгон оруулна уу.

Хэлэлцүүлэг

(0)

Нэвтрэх хэлэлцүүлэгт нэгдэхийн тулд

Сэтгэгдлүүдийг ачаалж байна...