Oriented Barium Ferrite Disc Magnet: Binder Dried in a 2400 Oersted Field (Gorter, Philips 1956, Ex. 3)

A ceramic magnet from pre-fired barium ferrite in polyvinyl acetate and acetone, dried in a 2400 oersted field, then pressed, heated and sintered as in Example 2. In the principal direction it held 2,720 gauss with a coercive force of 1,620 oersted and a (BH)max of 1.2 × 10⁶; at right angles 1,610 gauss. Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 3. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Дээд шат
3 days

Зааварчилгаа

1

Weigh barium carbonate and iron oxide

Weigh 450 g barium carbonate and 2000 g ferric oxide. Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Энэ алхмын материал:

Барийн карбонат (витерит)Барийн карбонат (витерит)450 г
Төмрийн (III) исэлТөмрийн (III) исэл2000 г

Шаардлагатай багаж:

Дэнсний жинлүүрДэнсний жинлүүр
Резинэн бээлийРезинэн бээлий
P100 амьсгалын хамгаалалтP100 амьсгалын хамгаалалт
2

Mill 20 hours under alcohol, dry

Grind the mixture in a ball mill under alcohol for 20 hours, then dry it.

Шаардлагатай багаж:

Төмөр бөмбөлөгт тээрэмТөмөр бөмбөлөгт тээрэм
Этанол - лабораторийн зэрэглэл, 95 %Этанол - лабораторийн зэрэглэл, 95 %
Хатаах зуухХатаах зуух
3

Pre-fire: through a 1100 °C zone in 10 minutes

Pass the dry powder at 20 mm per minute through an electric furnace with a 20 cm hot zone at 1100 °C, in air: 10 minutes in the heat. Let it cool.

Шаардлагатай багаж:

Хоолойн зуухХоолойн зуух
Тагтай хайлуур (шаазан)Тагтай хайлуур (шаазан)
Халуунд тэсвэртэй бээлийХалуунд тэсвэртэй бээлий
4

Grind 12 hours with alcohol, dry

Pulverise the pre-fired material in a ball mill with alcohol for 12 hours, then dry it. This is the pre-fired powder.

Шаардлагатай багаж:

Төмөр бөмбөлөгт тээрэмТөмөр бөмбөлөгт тээрэм
Этанол - лабораторийн зэрэглэл, 95 %Этанол - лабораторийн зэрэглэл, 95 %
Хатаах зуухХатаах зуух
5

Stir into 8 % polyvinyl acetate in acetone

Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 2 cc of solution per gram of powder. The binder burns off later.

Шаардлагатай багаж:

Поливинил ацетатПоливинил ацетат
АцетонАцетон
Дэнсний жинлүүрДэнсний жинлүүр
6

Orient in a 2400 oersted field

Put the suspension in a moulding die between the poles of a magnet and apply a first field of 2400 oersted. Remove the binder solution while the field is on.

Шаардлагатай багаж:

Диск шахах хэвДиск шахах хэв
ЭлектромагнитЭлектромагнит
Гидравлик прессГидравлик пресс
7

Compress into a block

Compress the powder into a block as in Example 2. The pressure is not given.

Шаардлагатай багаж:

Гидравлик прессГидравлик пресс
Диск шахах хэвДиск шахах хэв
8

Heat to 500 °C in a 2000 oersted field

Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.

Шаардлагатай багаж:

Хоолойн зуухХоолойн зуух
ЭлектромагнитЭлектромагнит
Халуунд тэсвэртэй бээлийХалуунд тэсвэртэй бээлий
9

Sinter: through a 1300 °C zone in 5 minutes

Pass the block at 20 mm per minute through an electric furnace in air at 1300 °C with a 10 cm hot zone: about 5 minutes in the heat.

Шаардлагатай багаж:

Хоолойн зуухХоолойн зуух
Халуунд тэсвэртэй бээлийХалуунд тэсвэртэй бээлий
10

Magnetise in the principal direction

Magnetise the block along the direction of the first field, the principal direction. The patent magnetises it in a field in that direction; ours: an electromagnet. Find the north face with a compass.

Шаардлагатай багаж:

ЭлектромагнитЭлектромагнит
Луужин (компас)Луужин (компас)

Материал

2

Шаардлагатай багаж

15

Энэ загвараар хийдэг

Холбоотой загварууд

Эдгээр загварууд мэдлэг хуваалцдаг — арга техник, материал эсвэл зарчим

CC0 Нийтийн домэйн

Энэ загвар CC0 дор гаргагдсан. Та зөвшөөрөл авахгүйгээр хуулах, өөрчлөх, түгээх, ашиглах боломжтой.

Загвараар дамжуулан бүтээгдэхүүн худалдаж авч Бүтээгчийг дэмжээрэй Бүтээгчийн шимтгэл Борлуулагчаар тогтоосон, эсвэл энэ загварын шинэ хувилбар үүсгэж орлогоо хуваахын тулд өөрийн загварт холбоос болгон оруулна уу.

Хэлэлцүүлэг

(0)

Нэвтрэх хэлэлцүүлэгт нэгдэхийн тулд

Сэтгэгдлүүдийг ачаалж байна...