Polypropylene Felt: a Spunbonded Web, Kinney 1967
Tex

Зохиогч

Tex

18. Аравдугаар сар 2026FO
7
0
0
0
0

Polypropylene Felt: a Spunbonded Web, Kinney 1967

A polypropylene felt made without weaving or needling: hot filaments are spun, pulled down by an air jet, given an electric charge so they spread apart, and laid in loops on a moving table until they form an even sheet. Kinney's patent (Du Pont, US 3,338,992, 1967) gives every setting for polypropylene. The corona runs at 20 to 25 kV: keep clear of it while it is live. The picture: the patent's own Fig. 1 (the process) and Fig. 7 (the web).
Дээд шат
1 day

Зааварчилгаа

1

Melt and spin

Melt polypropylene of melt index 10 in a screw extruder, no hotter than 290 °C. Meter it at 12 g a minute through a 1/4 in. sand filter and a 20-hole spinneret (holes 0.015 in. across): pack block 275 °C, spinneret 260 °C.

Энэ алхмын материал:

Полипропиленийн мөхлөгПолипропиленийн мөхлөг500 г

Шаардлагатай багаж:

Хуванцрын экструдерХуванцрын экструдер
ФильерФильер
ПирометрПирометр
Дэнсний жинлүүрДэнсний жинлүүр
Арьсан бээлийАрьсан бээлий
2

Quench

Cool the bundle of filaments in a 6 in. quench chimney blowing 40 cubic feet a minute of room air in from the side.

Шаардлагатай багаж:

Агаар шахагчАгаар шахагч
3

Draw with the air jet

Lead the bundle 72 in. down into an air draw jet run at 25 psi: it pulls the filaments with about 3 g of tension and stretches them.

Шаардлагатай багаж:

Агаараар сунгах цоргоАгаараар сунгах цорго
Агаар шахагчАгаар шахагч
Даралтын хэмжүүрДаралтын хэмжүүр
4

Charge the filaments

8 in. above the jet, let the filaments brush a 1 1/4 in. bar turning at 10 rpm, with a four-point corona 5/8 in. from it at minus 20 to 25 kV (100 to 150 µA). The charge pushes them apart. Keep clear while it is live.

Шаардлагатай багаж:

Коронаар цэнэглэх төхөөрөмжКоронаар цэнэглэх төхөөрөмж
5

Lay the web

Catch the filaments on a grounded 47 in. square table that moves 26 in. a minute one way and 570 in. a minute the other. Each layer weighs 0.5 oz per square yard; lay several for each sheet.

Шаардлагатай багаж:

Дэвсэх ширээДэвсэх ширээ
6

What you get

An even sheet of fine filaments, about 2.5 denier each, tenacity 2.0 g per denier, stretching 300 % before they break.

Шаардлагатай багаж:

Дэнсний жинлүүрДэнсний жинлүүр

Материал

1

Шаардлагатай багаж

10

CC0 Нийтийн домэйн

Энэ загвар CC0 дор гаргагдсан. Та зөвшөөрөл авахгүйгээр хуулах, өөрчлөх, түгээх, ашиглах боломжтой.

Загвараар дамжуулан бүтээгдэхүүн худалдаж авч Бүтээгчийг дэмжээрэй Бүтээгчийн шимтгэл Борлуулагчаар тогтоосон, эсвэл энэ загварын шинэ хувилбар үүсгэж орлогоо хуваахын тулд өөрийн загварт холбоос болгон оруулна уу.

Хэлэлцүүлэг

(0)

Нэвтрэх хэлэлцүүлэгт нэгдэхийн тулд

Сэтгэгдлүүдийг ачаалж байна...