Porcelain Labware: Evaporating Dishes, Crucibles, Funnels and Streak Plates
Hard porcelain stands strong heat and most chemicals, so the laboratory's dishes, crucibles and filter funnels are made of it; left unglazed, its white biscuit is the streak plate for testing minerals. Form the pieces, give them a light first firing, dip them in ground-felspar glaze, and fire them hard in saggers, as Andrew Ure (1839) describes for Sèvres.
The picture: porcelain evaporating dishes in three sizes, glazed, with pouring lips.
Дээд шат
Weeks with drying and two firings
Зааварчилгаа
1
1
Form the pieces
Form the pieces
Throw shallow round dishes with a lip and small lidded crucibles on the wheel. For a Büchner funnel throw a cylinder with a flat floor, pierce the floor with many small holes and add a stem. Roll a slab and cut it into small tiles for streak plates.
Энэ алхмын материал:
Шаазангийн шавар5 кгШаардлагатай багаж:
Ваарчны хүрд
Гурил дэлгэгч бул
Ваарны багажны багц
Шугам2
2
Dry very slowly
Dry very slowly
Ure: dry them very slowly; a little hurry spoils them.
3
3
Light first firing
Light first firing
Fire them gently so they keep their shape but become strong enough to handle and be dipped in water.
Энэ алхмын материал:
Түлээ1 as requiredШаардлагатай багаж:
Шатаах зуух
Халуунд тэсвэртэй бээлий4
4
Felspar glaze
Felspar glaze
Grind felspar very fine, stir it with water and a little vinegar to a thin pap. Dip each dish, crucible and funnel for an instant; the porous body draws the glaze on. Wipe the glaze off the feet. Leave the streak-plate tiles unglazed.
Энэ алхмын материал:
Хээрийн жоншны хэсэг0.5 кг
Ус2 литр
Цуу0.05 литрШаардлагатай багаж:
Нунтаглагч чулуу
Нарийн тортой шигшүүр
Модон том сав
Тоосны маск5
5
Set in saggers
Set in saggers
Set every piece in its own sagger on a flat, sand-dusted base so it cannot stick or sag out of shape; small pieces may share a base if they do not touch.
Энэ алхмын материал:
Нарийн элс1 кгШаардлагатай багаж:
Галд тэсвэртэй хайрцаг (саггер)6
6
The hard firing
The hard firing
Raise the fire slowly for about 15 hours to a cherry red, then fire hard until the kiln glows white inside, drawing trial pieces to judge when the glaze is smooth. Cool slowly over days.
Энэ алхмын материал:
Түлээ1 as requiredШаардлагатай багаж:
Шатаах зуух
Халуунд тэсвэртэй бээлий7
7
Ure's firing, hour by hour
Ure's firing, hour by hour
Jupyter дэвтэр ачаалж байна…
8
8
Limits
Limits
The firings, glaze and saggers are Ure's account of Sèvres; the forms of the four wares are ours. A full porcelain firing needs a kiln that reaches white heat.
Материал
6- 5 кгТүр орлуулагч
- 1 as requiredТүр орлуулагч
- 0.5 кгТүр орлуулагч
- 2 литрТүр орлуулагч
- 0.05 литрТүр орлуулагч
- 1 кгТүр орлуулагч
Шаардлагатай багаж
11- Түр орлуулагч
- Түр орлуулагч
- Түр орлуулагч
- Түр орлуулагч
- Түр орлуулагч
- Түр орлуулагч
- Түр орлуулагч
- Түр орлуулагч
- Түр орлуулагч
- Түр орлуулагч
- Түр орлуулагч
Энэ загвараар хийдэг
Холбоотой загварууд
Эдгээр загварууд мэдлэг хуваалцдаг — арга техник, материал эсвэл зарчим
CC0 Нийтийн домэйн
Энэ загвар CC0 дор гаргагдсан. Та зөвшөөрөл авахгүйгээр хуулах, өөрчлөх, түгээх, ашиглах боломжтой.
Загвараар дамжуулан бүтээгдэхүүн худалдаж авч Бүтээгчийг дэмжээрэй Бүтээгчийн шимтгэл Борлуулагчаар тогтоосон, эсвэл энэ загварын шинэ хувилбар үүсгэж орлогоо хуваахын тулд өөрийн загварт холбоос болгон оруулна уу.