Reverberatory Furnace: the Air Furnace for Melting Cast Iron (Bolland, 1893)
An air furnace melts iron apart from the fuel: coal burns on a grate at one end, and the flame is thrown down from a low arched roof onto the iron on the bed, then leaves by a tall chimney. The iron stays cleaner than in a cupola, so founders used it for guns, rolls, heavy scrap and lumps too big for the cupola.
This furnace is 30 ft 6 in long and 7 ft wide outside, 5 ft wide inside, cased in bolted wrought-iron plates.
Source: S. Bolland, The Iron Founder Supplement (1893), pp. 55-67. Unknown: brick sizes, plate thickness. Picture: Fig. 14 of the book.
Мэргэжилтэн
Unknown
Зааварчилгаа
1
1
Lay the foundation
Lay the foundation
Build the foundation solid of common material up to the firebrick, shaped so the firebrick bed slopes down from the chimney end to the reservoir. Keep the bricks from B to C 6 in below the finished bottom, to leave room for the sand bed.
Энэ алхмын материал:
Тоосго1 foundationШаардлагатай багаж:
Барилгын халбага (шпатель)
Тодорхойгүй хэмжээс2
2
Build the fireplace, bridge and roof
Build the fireplace, bridge and roof
Build the fireplace the full width of the furnace (5 ft inside, grate 5 ft long). Set the bridge wall at least 2 ft 3 in from the face of the grate bars. Build bridge, sides, roof and fireplace of the most refractory firebrick. Arch the roof the whole length, low, so it throws the flame down onto the bed; fill above the arches with common material. Leave the side charging hole (5 x 4 ft), the top hole (furnace width x 6 ft), the puddling hole over the reservoir, a sight hole and the tap hole.
Энэ алхмын материал:
Галд тэсвэртэй шавран тоосго1 lining, bridge, roof
Галд тэсвэртэй шавран зуурмаг1 setting
Тоосго1 filling above the arch
Тодорхойгүй металл1 grate barsШаардлагатай багаж:
Барилгын халбага (шпатель)3
3
Case it in plates and bolt it
Case it in plates and bolt it
Case the whole structure in wrought-iron plates, held at the corners with angle-irons. Run eight chief anchor bolts from side to side, clear of all working parts. Join everything with bolts, not rivets, so any plate can come off for repairs. Line the charging doors with firebrick.
Энэ алхмын материал:
Төмөр хавтан1 casing, doors
Давтмал төмрийн саваа8 anchor bolts
Тодорхойгүй металл1 angle-irons, door frames
Галд тэсвэртэй шавран тоосго1 door liningsШаардлагатай багаж:
Тодорхойгүй хэмжээс4
4
Build the chimney
Build the chimney
Build the chimney square, 30 to 40 ft high, with an inside course of firebrick (Fig. 14: 2 ft 6 in square inside). Make its area a little larger than the fireplace. Put a damper on top that can be worked from the bottom: it alone sets the draught. It can stand apart on a sole plate on four columns.
Энэ алхмын материал:
Галд тэсвэртэй шавран тоосго1 inside course
Тоосго1 chimney
Тодорхойгүй металл1 damperШаардлагатай багаж:
Барилгын халбага (шпатель)5
5
Make the sand bottom
Make the sand bottom
Make the bottom from B round the reservoir to C with 8 parts fire-sand to 1 of clay and 1 of ground coke. Fire it well for one to two hours before the first charge; it should last ten heats. Fill the tap hole with fire-sand and a little coal dust, which will not cake when hot.
Энэ алхмын материал:
Элс8 parts
Шавар1 part
Металлургийн кокс1 part, groundШаардлагатай багаж:
Битумэн нүүрс6
6
Charge and melt
Charge and melt
Fire with soft, non-caking bituminous coal and keep a full grate; clinker quickly and leave no holes for cold air. Charge all the iron at the start: first layer of pigs lengthwise and a little apart, next layers across, open so the flame passes. Set heavy pieces on firebricks so the flame plays all round them. Through the puddling hole, dip test pieces and skim the iron clean. To blend two grades, thrust green saplings into the melt. Close the damper before tapping. Look the furnace over after every heat.
Шаардлагатай багаж:
Битумэн нүүрс
Цутгамал төмрийн гулдмай
Хатуу модны залуу мөчир
Нүхтэй шөл авагчМатериал
9- 1 chimneyТүр орлуулагч
- 1 inside courseТүр орлуулагч
- 1 settingТүр орлуулагч
- 1 damperТүр орлуулагч
- 1 casing, doorsТүр орлуулагч
- 8 anchor boltsТүр орлуулагч
- 8 partsТүр орлуулагч
- 1 partТүр орлуулагч
- 1 part, groundТүр орлуулагч
Шаардлагатай багаж
6- Түр орлуулагч
- Түр орлуулагч
- Түр орлуулагч
- Түр орлуулагч
- Түр орлуулагч
- Түр орлуулагч
Холбогдсон загварын материал

10% хамаарал
Fireclay Firebricks
Clay зохиосон
Керамик ба шавар
39
0
0
0
4
0

10% хамаарал
Cupola Furnace: the Common Foundry Cupola with a Drop Bottom (Bolland, 1893)
Forge зохиосон
Зуух
9
0
0
0
1
0

10% хамаарал
Making Coke from Coal — The Smokeless Fuel That Forged the Industrial Revolution
Gimli зохиосон
Металл боловсруулалт
73
0
0
0
4
0
Энэ загвараар хийдэг
CC0 Нийтийн домэйн
Энэ загвар CC0 дор гаргагдсан. Та зөвшөөрөл авахгүйгээр хуулах, өөрчлөх, түгээх, ашиглах боломжтой.
Загвараар дамжуулан бүтээгдэхүүн худалдаж авч Бүтээгчийг дэмжээрэй Бүтээгчийн шимтгэл Борлуулагчаар тогтоосон, эсвэл энэ загварын шинэ хувилбар үүсгэж орлогоо хуваахын тулд өөрийн загварт холбоос болгон оруулна уу.