Rubber Stoppers: Pará Rubber with Ceresine, Moulded and Cured (Heil & Esch 1909)
Heil and Esch · Public domain (1909)
Emma

Зохиогч

Emma

27. Аравдугаар сар 2026SE
15
0
0
0
0

Rubber Stoppers: Pará Rubber with Ceresine, Moulded and Cured (Heil & Esch 1909)

Laboratory rubber stoppers from a 1909 rubber factory's book of mixings: Pará rubber with ceresine wax, sulphur and magnesia, run out as a cord, cut to weight, pressed into moulds and cured. Source: Heil & Esch, The Manufacture of Rubber Goods (1909), mixing No. 34 (p. 108) and the stopper method (p. 135). They give no cure time or temperature. Using smoked ball rubber as their Pará, and the mill, clamps and steam vessel, are ours. Picture: their page of mixings.
Дунд шат
1 day

Зааварчилгаа

1

Weigh mixing No. 34

Weigh out 10,000 g Pará rubber, 2,000 g ceresine, 1,000 g sulphur and 100 g calcined magnesia (magnesia usta).

Энэ алхмын материал:

Утсан резинэн бөмбөгУтсан резинэн бөмбөг10000 г
Церезин лавЦерезин лав2000 г
Хүхрийн нунтагХүхрийн нунтаг1000 г
Магнийн исэлМагнийн исэл100 г

Шаардлагатай багаж:

Дэнсний жинлүүрДэнсний жинлүүр
2

Mix on the rolls

Work the rubber on the mixing rolls and work the ceresine, sulphur and magnesia into it until the mixing is even.

Шаардлагатай багаж:

Хоёр булт резин нухагчХоёр булт резин нухагч
3

Run a cord on the tube machine

Run the mixing through the tube machine as a cord of a size to suit the stoppers. It must be free from air bubbles, or the stoppers will be faulty after curing.

Шаардлагатай багаж:

Резин хоолой шахах машинРезин хоолой шахах машин
4

Cut pieces to weight

Cut the cord into pieces of the exact weight of one stopper plus 2 or 3 per cent, for what squeezes out of the mould.

Шаардлагатай багаж:

Гар урлалын хутгаГар урлалын хутга
Дэнсний жинлүүрДэнсний жинлүүр
5

Press into moulds and clamp

Press each piece into a mould and clamp the small moulds very tightly in iron clips.

Шаардлагатай багаж:

Вулканжуулах хэвВулканжуулах хэв
C хэлбэрийн хавчаарC хэлбэрийн хавчаар
6

Cure in steam

Cure the clamped moulds in a steam heater (Heil & Esch also name the sulphur bath). They give no time or temperature for stoppers; then open the moulds and take out the stoppers.

Шаардлагатай багаж:

Ширээний автоклавШирээний автоклав
Вулканжуулах хэвВулканжуулах хэв

Материал

4

Шаардлагатай багаж

7

Холбоотой загварууд

Эдгээр загварууд мэдлэг хуваалцдаг — арга техник, материал эсвэл зарчим

CC0 Нийтийн домэйн

Энэ загвар CC0 дор гаргагдсан. Та зөвшөөрөл авахгүйгээр хуулах, өөрчлөх, түгээх, ашиглах боломжтой.

Загвараар дамжуулан бүтээгдэхүүн худалдаж авч Бүтээгчийг дэмжээрэй Бүтээгчийн шимтгэл Борлуулагчаар тогтоосон, эсвэл энэ загварын шинэ хувилбар үүсгэж орлогоо хуваахын тулд өөрийн загварт холбоос болгон оруулна уу.

Хэлэлцүүлэг

(0)

Нэвтрэх хэлэлцүүлэгт нэгдэхийн тулд

Сэтгэгдлүүдийг ачаалж байна...