Thulium: Oxide Reduced with Aluminium in Flowing Argon and the Vapour Condensed (CN 104152695 B)
Pellets of thulium oxide and aluminium are fed into an induction furnace at 1700 °C. The aluminium takes the oxygen and stays behind as slag. Thulium boils off as vapour, and a stream of argon carries it into a water-cooled tank where it condenses to metal.
Result: thulium metal, 99.5 % of the thulium recovered. No vacuum pump is needed: the moving argon sweeps the vapour away as fast as it forms.
Source: Zhang, Dou et al. (Northeastern University), Chinese patent CN 104152695 B (2014), Example 1. Not given: batch size, the form of the aluminium, pellet size, the purity of the thulium. Picture: Wikimedia Commons.
Дээд шат
1 day
Зааварчилгаа
1
1
Weigh and mix
Weigh and mix
Weigh thulium oxide and aluminium, both over 99.0 % pure, in the molar ratio 1 : 2.2: 10 % more aluminium than the reaction needs (ours: about 15.4 g of aluminium to 100 g of oxide). Mix them evenly.
Энэ алхмын материал:
Тулийн исэл100 гШаардлагатай багаж:
Хөнгөн цагаан
Жин2
2
Press into pellets
Press into pellets
Press the mix in a roller press at 100 kg/cm² into lumpy pellets.
Шаардлагатай багаж:
Галзуурт пресс3
3
Reduce in flowing argon
Reduce in flowing argon
Run argon (99.95 %) through a medium-frequency induction furnace (the patent's coil is 220 mm across) at 5 L/min; ours: set the flow with a rotameter. Feed the pellets in continuously and hold them at 1700 °C for 30 min. The thulium leaves as vapour mixed with the argon; draw the slag off continuously.
Шаардлагатай багаж:
Индукцийн хайлуулах зуух
Аргон
Ротаметр4
4
Condense the thulium
Condense the thulium
Let the argon carry the vapour out of the furnace through a sealed pipe straight into a condensing tank cooled by circulating water. The thulium condenses there as metal: 99.5 % recovered. Example 2 of the patent runs at 1500 °C for 60 min with 15 L/min of argon (pellets pressed at 150 kg/cm²) and reports 99.2 %.
Шаардлагатай багаж:
Конденсацийн камер
УсМатериал
1- 100 гТүр орлуулагч
Энэ загвараар хийдэг
Холбоотой загварууд
Эдгээр загварууд мэдлэг хуваалцдаг — арга техник, материал эсвэл зарчим

Аюултай
Erbium, Ytterbium, Thulium and Lutetium Oxides: Xenotime Separated on Ion Exchange Columns with EDTA and HEDTA (Spedding and Powell, US 2,956,858)
Charlie зохиосон
Органик бус
8
0
0
0
0
0

Аюултай
Aluminium by Hall–Héroult Electrolysis: Alumina in Molten Cryolite
Forge зохиосон
Металл боловсруулалт
6
0
0
0
0
0

Argon: Air Led over Calcium Carbide and Calcium Chloride at 800 °C (Fischer and Ringe, Thorpe 1912)
Charlie зохиосон
Органик бус
8
0
0
0
0
0

Ytterbium: Oxide Reduced by Lanthanum at 1020 °C in Vacuum, Metal Distilled Off (Shindo and Yagi, US 2010/0260640)
Charlie зохиосон
Органик бус
7
0
0
0
0
0
CC0 Нийтийн домэйн
Энэ загвар CC0 дор гаргагдсан. Та зөвшөөрөл авахгүйгээр хуулах, өөрчлөх, түгээх, ашиглах боломжтой.
Загвараар дамжуулан бүтээгдэхүүн худалдаж авч Бүтээгчийг дэмжээрэй Бүтээгчийн шимтгэл Борлуулагчаар тогтоосон, эсвэл энэ загварын шинэ хувилбар үүсгэж орлогоо хуваахын тулд өөрийн загварт холбоос болгон оруулна уу.