White Charcoal Pig Iron: Calcined Magnetic Ore Smelted with Charcoal in a Swedish Blast Furnace (Percy, 1864)
Forge

Зохиогч

Forge

1. Арван нэгдүгээр сар 2026NO
7
0
0
0
0

White Charcoal Pig Iron: Calcined Magnetic Ore Smelted with Charcoal in a Swedish Blast Furnace (Percy, 1864)

Sweden's bar iron began in small charcoal blast furnaces fed with roasted magnetic ore. Percy describes the Sten furnace and how the Swedes smelted: slow, with gentle blast, and with no hot blast at all for the best Dannemora iron, whose manganese-rich ore gives a white, crystalline pig made for the finery. Result: white pig iron in iron moulds, 40-60 tons a week; about half the weight of the ore comes out as iron. Source: John Percy, Metallurgy: Iron and Steel (1864), pp. 370-375. Picture: Percy's Fig. 54, the Swedish blast furnace.
Мэргэжилтэн
continuous; tapped every 6 hours

Зааварчилгаа

1

Calcine the ore

Break the magnetic ore into lumps no bigger than a double fist and roast it carefully in a mine-kiln heated by the waste gas of the furnace. The Swedes always calcine mountain ores, even without sulphur; any sulphur from pyrites is driven off.

Энэ алхмын материал:

МагнетитМагнетит1 ore

Шаардлагатай багаж:

Шарах зуухШарах зуух
2

Crush the roasted ore

Crush the calcined ore between grooved cast-iron rolls driven by an overshot water wheel, to pieces of ¼ to 1 cubic inch.

Шаардлагатай багаж:

Бутлах булнуудБутлах булнууд
Усан хүрдУсан хүрд
3

Prepare the furnace

Use a charcoal blast furnace of fire-brick in a sand-filled outer shell. Stamp the lower boshes and hearth from 6 parts crushed quartz to 1 part raw fire-clay by measure round a wooden block, and dry it very slowly with a wood fire. It has three water-cooled tuyeres about 2½ inches across.

Шаардлагатай багаж:

Домен зуухДомен зуух
4

Set the blast

Blow with a water-driven blowing engine (at Sten three cylinders about 45 inches across, 45-inch stroke) at ½ to 1½ lb per square inch, more for hard charcoal. Keep the blast so slow that the furnace contents take at least 12 hours to pass through. For pig meant for bar iron the blast is warmed only to about 100 °C; the best Dannemora iron is made with cold blast.

Шаардлагатай багаж:

Үлээлгэх машинҮлээлгэх машин
Усан хүрдУсан хүрд
5

Charge charcoal and ore

Charge 30-50 cubic feet of charcoal at a time and 7-10 cwt of ore on top, half spread round the sides and half in the middle, the most siliceous ore first. Dannemora ore needs no flux (other ores take 10-15 % limestone). It takes about 0.8 to 1 ton of charcoal per ton of iron.

Энэ алхмын материал:

Модны нүүрсМодны нүүрс1 0.8-1 ton per ton of iron

Шаардлагатай багаж:

Домен зуухДомен зуух
6

Tap into iron moulds

Tap every 6 hours and run the metal into iron moulds, not sand. A furnace makes 40-60 tons a week; the cinder runs thin and holds under 1 % iron. Pig from Dannemora ore is white and crystalline, from its manganese.

Шаардлагатай багаж:

Гулдмайн хэвГулдмайн хэв

Материал

2
  • Түр орлуулагч
  • 1 0.8-1 ton per ton of iron
    Түр орлуулагч

Шаардлагатай багаж

6

Холбоотой загварууд

Эдгээр загварууд мэдлэг хуваалцдаг — арга техник, материал эсвэл зарчим

CC0 Нийтийн домэйн

Энэ загвар CC0 дор гаргагдсан. Та зөвшөөрөл авахгүйгээр хуулах, өөрчлөх, түгээх, ашиглах боломжтой.

Загвараар дамжуулан бүтээгдэхүүн худалдаж авч Бүтээгчийг дэмжээрэй Бүтээгчийн шимтгэл Борлуулагчаар тогтоосон, эсвэл энэ загварын шинэ хувилбар үүсгэж орлогоо хуваахын тулд өөрийн загварт холбоос болгон оруулна уу.

Хэлэлцүүлэг

(0)

Нэвтрэх хэлэлцүүлэгт нэгдэхийн тулд

Сэтгэгдлүүдийг ачаалж байна...