Barium-Calcium Ferrite Disc Magnet: 20 % Calcium, 5 Minutes at 1290 °C (Went, Philips 1956, Ex. 20)
A ceramic magnet with a fifth of the barium replaced by calcium: 0.08 mol barium carbonate, 0.02 mol calcium carbonate and 0.6 mol iron oxide, made as in Example 18 but sintered at 1290 °C for only 5 minutes. Went's rod held 1,615 gauss with a coercive force of 1,550 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 20. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Lanjutan
2 days
Arahan
1
1
Weigh barium carbonate, chalk and iron oxide
Weigh barium carbonate, chalk and iron oxide
Weigh 15.79 g barium carbonate (0.08 mol), 2.002 g calcium carbonate (0.02 mol) and 95.55 g ferric oxide (0.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.
Bahan untuk langkah ini:
Barium karbonat (witherit)15.79 g
Kalsium karbonat (kapur putih halus)2.002 g
Ferik Oksida95.55 gAlatan diperlukan:
Neraca dua piring
Sarung tangan getah
Alat Pernafasan P1002
2
Mill, presinter and mill as in Example 18
Mill, presinter and mill as in Example 18
As in Example 18: grind with alcohol 4 hours, dry at 150 °C, fire in air at 1000 °C for 2 hours, grind again 4 hours and dry.
Alatan diperlukan:
Kilang Bebola Besi
Etanol mutu makmal, 95 %
Ketuhar pengeringan
Relau Muffle
Mangkuk pijar bertutup (porselin)
Penyepit Mangkuk Pijar3
3
Press at 1.5 t/cm²
Press at 1.5 t/cm²
Press at 1.5 tonnes per cm², as in Example 18 (ours: discs instead of rods).
Alatan diperlukan:
Mesin tekan hidraulik
Acuan tekan cakera4
4
Pass through a 1290 °C zone in 5 minutes
Pass through a 1290 °C zone in 5 minutes
Sinter in air at 1290 °C by passing the pieces through a 10 cm hot zone at 20 mm per minute: 5 minutes in the heat.
Alatan diperlukan:
Relau Tiub
Sarung Tangan Tahan Haba5
5
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
Alatan diperlukan:
Elektromagnet
KompasBahan
3- 15.79 gPemegang Tempat
- Pemegang Tempat
- 95.55 gPemegang Tempat
Alatan Diperlukan
15- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
Blueprint ini membuat
Blueprint berkaitan
Blueprint ini berkongsi pengetahuan — teknik, bahan atau prinsip
CC0 Domain Awam
Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.
Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.