Barium-Calcium Ferrite Disc Magnet: Equal Barium and Calcium, Sintered at 1280 °C (Went, Philips 1956, Ex. 22)
A ceramic magnet with equal parts barium and calcium: 0.3 mol barium carbonate, 0.3 mol calcium carbonate and 3.1 mol iron oxide, milled 15 hours, pressed and passed through a 1280 °C furnace in 10 minutes, with no presintering. Went's rod held 1,595 gauss with a coercive force of 1,890 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 22. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Lanjutan
2 days
Arahan
1
1
Weigh barium carbonate, chalk and iron oxide
Weigh barium carbonate, chalk and iron oxide
Weigh 59.5 g barium carbonate (0.3 mol), 30.2 g calcium carbonate (0.3 mol) and 500.0 g ferric oxide (3.1 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.
Bahan untuk langkah ini:
Barium karbonat (witherit)59.5 g
Kalsium karbonat (kapur putih halus)30.2 g
Ferik Oksida500 gAlatan diperlukan:
Neraca dua piring
Sarung tangan getah
Alat Pernafasan P1002
2
Mill with alcohol 15 hours, dry, press
Mill with alcohol 15 hours, dry, press
Grind with alcohol in a ball mill for 15 hours, dry, and press at 1.5 tonnes per cm² (ours: discs instead of rods). No presintering.
Alatan diperlukan:
Kilang Bebola Besi
Etanol mutu makmal, 95 %
Ketuhar pengeringan
Mesin tekan hidraulik
Acuan tekan cakera3
3
Pass through a 1280 °C zone in 10 minutes
Pass through a 1280 °C zone in 10 minutes
Sinter at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.
Alatan diperlukan:
Relau Tiub
Sarung Tangan Tahan Haba4
4
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
Alatan diperlukan:
Elektromagnet
KompasBahan
3- Pemegang Tempat
- Pemegang Tempat
- 500 gPemegang Tempat
Alatan Diperlukan
12- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
Blueprint ini membuat
Blueprint berkaitan
Blueprint ini berkongsi pengetahuan — teknik, bahan atau prinsip
CC0 Domain Awam
Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.
Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.