Barium Ferrite Disc Magnet: Fired in Carbon Dioxide, Pressed at 12 t/cm² (Went, Philips 1956, Ex. 33)
Charlie

Dicipta oleh

Charlie

28. Oktober 2026DE
6
0
0
0
0

Barium Ferrite Disc Magnet: Fired in Carbon Dioxide, Pressed at 12 t/cm² (Went, Philips 1956, Ex. 33)

A barium ferrite made with more iron oxide, 0.4 mol barium carbonate to 3.6 mol, fired an hour at 1300 °C in carbon dioxide. Little oxygen gives the hexagonal crystal BaFe18O27, with some iron in the lower state. It is milled again, bound with nitrocellulose or polyvinyl alcohol, and pressed hard at 12 tonnes per cm². Went's rod held 1,260 gauss with a coercive force of 700 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 33. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Lanjutan
2 days

Arahan

1

Weigh barium carbonate and iron oxide

Weigh 79.4 g barium carbonate (0.4 mol) and 580.9 g ferric oxide (3.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Bahan untuk langkah ini:

Barium karbonat (witherit)Barium karbonat (witherit)79.4 g
Ferik OksidaFerik Oksida580.9 g

Alatan diperlukan:

Neraca dua piringNeraca dua piring
Sarung tangan getahSarung tangan getah
Alat Pernafasan P100Alat Pernafasan P100
2

Mill 15.5 hours, press a pastille, fire in CO2

Grind with alcohol in a ball mill for 15.5 hours, dry, and press into a pastille. Heat it at 1300 °C in carbon dioxide for 1 hour (ours: a tube furnace fed from a CO2 cylinder).

Alatan diperlukan:

Kilang Bebola BesiKilang Bebola Besi
Etanol mutu makmal, 95 %Etanol mutu makmal, 95 %
Ketuhar pengeringanKetuhar pengeringan
Mesin tekan hidraulikMesin tekan hidraulik
Acuan tekan cakeraAcuan tekan cakera
Relau TiubRelau Tiub
Gas karbon dioksidaGas karbon dioksida
Silinder gas bertekananSilinder gas bertekanan
Sarung Tangan Tahan HabaSarung Tangan Tahan Haba
3

Pulverise, mill 14 hours, bind

Crush the cooled pastille and grind it with alcohol for 14 hours. Press the powder into a pastille again with a ceramic binder (ours: polyvinyl alcohol, one of the two named), then crush it to grains.

Bahan untuk langkah ini:

Serbuk polivinil alkoholSerbuk polivinil alkohol1 as required

Alatan diperlukan:

Kilang Bebola BesiKilang Bebola Besi
Etanol mutu makmal, 95 %Etanol mutu makmal, 95 %
Mesin tekan hidraulikMesin tekan hidraulik
Acuan tekan cakeraAcuan tekan cakera
4

Press at 12 tonnes per cm²

Press the grains at 12 tonnes per cm² (ours: discs instead of rods). The patent describes no further firing.

Alatan diperlukan:

Mesin tekan hidraulikMesin tekan hidraulik
Acuan tekan cakeraAcuan tekan cakera
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Alatan diperlukan:

ElektromagnetElektromagnet
KompasKompas

Bahan

3

Alatan Diperlukan

14

Blueprint berkaitan

Blueprint ini berkongsi pengetahuan — teknik, bahan atau prinsip

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...