Barium Ferrite Disc Magnet, Sintered at 1300 °C (Went, Philips 1956)

The dark grey ceramic magnet on fridges and in loudspeakers is barium ferrite. It is made from two cheap powders: one part barium carbonate to six of iron oxide, milled, fired, milled again, pressed and sintered. No cobalt or nickel is needed. This is Example 34 of the Philips patent. This iteration sinters at 1300 °C, where his rod held 1,850 gauss with a coercive force of 1,780 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956). They pressed rods; the claim covers "a body of a desired shape", and the disc size is ours. The patent does not say how to magnetise it; our way is stated. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Lanjutan
2 days

Arahan

1

Weigh one part barium carbonate to six of iron oxide

Weigh 39.5 g of barium carbonate (0.2 mol) and 191.7 g of ferric oxide, Fe2O3 (1.2 mol). Barium carbonate is poisonous if swallowed: ours, gloves and a dust respirator.

Bahan untuk langkah ini:

Barium karbonat (witherit)Barium karbonat (witherit)39.5 g
Ferik OksidaFerik Oksida191.7 g

Alatan diperlukan:

Neraca dua piringNeraca dua piring
Sarung tangan getahSarung tangan getah
Alat Pernafasan P100Alat Pernafasan P100
2

Mill with ethanol for 4 hours

Grind the mixture with ethanol in an iron ball mill for 4 hours. Let the ethanol evaporate, then dry the powder in a drying oven.

Alatan diperlukan:

Kilang Bebola BesiKilang Bebola Besi
Etanol mutu makmal, 95 %Etanol mutu makmal, 95 %
Ketuhar pengeringanKetuhar pengeringan
3

Presinter at 1000 °C for 4 hours

Fire the dry powder in air at 1000 °C for 4 hours (ours: in a lidded porcelain crucible in a muffle furnace). Let it cool.

Alatan diperlukan:

Relau MuffleRelau Muffle
Mangkuk pijar bertutup (porselin)Mangkuk pijar bertutup (porselin)
Penyepit Mangkuk PijarPenyepit Mangkuk Pijar
Sarung Tangan Tahan HabaSarung Tangan Tahan Haba
4

Mill again for 4 hours

Grind the presintered product with ethanol in the ball mill for another 4 hours. Let the ethanol evaporate.

Alatan diperlukan:

Kilang Bebola BesiKilang Bebola Besi
Etanol mutu makmal, 95 %Etanol mutu makmal, 95 %
Ketuhar pengeringanKetuhar pengeringan
Alat Pernafasan P100Alat Pernafasan P100
5

Press discs at 1.5 tons per cm²

Press the powder at 1.5 tons/cm². The patent pressed rods; we press discs. Ours: a die 20 mm across, so about 4.7 tonnes on the punch (our arithmetic: 1.5 × 3.14 cm²).

Alatan diperlukan:

Mesin tekan hidraulikMesin tekan hidraulik
Acuan tekan cakeraAcuan tekan cakera
6

Sinter 4 hours at 1300 °C

Sinter the discs for 4 hours at 1300 °C in oxygen or in air. The patent's rod at 1300 °C: 1,850 gauss and 1,780 oersted.

Alatan diperlukan:

Relau MuffleRelau Muffle
Penyepit Mangkuk PijarPenyepit Mangkuk Pijar
Sarung Tangan Tahan HabaSarung Tangan Tahan Haba
7

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Alatan diperlukan:

ElektromagnetElektromagnet
KompasKompas

Bahan

2

Alatan Diperlukan

14

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...