Barium Ferrite Disc Magnet: 0.5 mol BaCO3 to 3.5 mol Iron Oxide, 10 Minutes at 1330 °C (Went, Philips 1956, Ex. 4)

A barium ferrite with much more iron oxide: 0.5 mol barium carbonate to 3.5 mol, milled 15.5 hours, bound, formed and sintered 10 minutes at 1330 °C. Went's rod held 2,040 gauss with a coercive force of 2,380 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 4. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Lanjutan
2 days

Arahan

1

Weigh barium carbonate and iron oxide

Weigh 99.2 g barium carbonate (0.5 mol) and 564.8 g ferric oxide (3.5 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Bahan untuk langkah ini:

Barium karbonat (witherit)Barium karbonat (witherit)99.2 g
Ferik OksidaFerik Oksida564.8 g

Alatan diperlukan:

Neraca dua piringNeraca dua piring
Sarung tangan getahSarung tangan getah
Alat Pernafasan P100Alat Pernafasan P100
2

Mill with alcohol 15.5 hours, dry and sieve

Grind the mixture with alcohol in a ball mill for 15.5 hours, then dry it and sieve it.

Alatan diperlukan:

Kilang Bebola BesiKilang Bebola Besi
Etanol mutu makmal, 95 %Etanol mutu makmal, 95 %
Ketuhar pengeringanKetuhar pengeringan
AyakAyak
3

Knead with a binder and form

Mix 300 g of the powder with a binder such as polyvinyl alcohol (Went names it or nitrocellulose) into a kneadable mass. The patent extrudes rods about 3 mm across; ours: press discs at 1.5 tonnes per cm², as in its other examples. Dry them in air for about 24 hours.

Alatan diperlukan:

Serbuk polivinil alkoholSerbuk polivinil alkohol
Mesin tekan hidraulikMesin tekan hidraulik
Acuan tekan cakeraAcuan tekan cakera
Ketuhar pengeringanKetuhar pengeringan
4

Sinter in air at 1330 °C for 10 minutes

Sinter the pieces in air at 1330 °C for 10 minutes. The patent gives no zone length or speed for this example.

Alatan diperlukan:

Relau TiubRelau Tiub
Sarung Tangan Tahan HabaSarung Tangan Tahan Haba
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Alatan diperlukan:

ElektromagnetElektromagnet
KompasKompas

Bahan

2

Alatan Diperlukan

14

Blueprint berkaitan

Blueprint ini berkongsi pengetahuan — teknik, bahan atau prinsip

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...