Ceramic rods tumble in a hot, gas-tight rotating furnace while methane cracks on them and leaves a thin, hard film of carbon. The coated rods get conducting ends, a helix ground through the film to bring them near their value, a light rub to the exact value, and a coat of baking varnish. Result: carbon film resistors adjusted to as close as ±0.5 %. The helix alone can raise a rod's resistance by any factor from about 10 to about 8000. Source: Grisdale, Pfister and van Roosbroeck, Pyrolytic Film Resistors, Bell System Technical Journal 30 (1951). Unknown: the ceramic of the rods, the end caps and leads, and which baking varnish; the paper does not give them. Picture: Wikimedia Commons.
Lanjutan
2 days

Arahan

1

Load the furnace

Load cylindrical ceramic rods into the gas-tight refractory core of a rotating (or rocking) batch furnace, with silica sand to support the rods and keep them from damage as they tumble. Unknown: which ceramic.

Bahan untuk langkah ini:

Teras penebat perintangTeras penebat perintang1 batch

Alatan diperlukan:

Relau berputar kelompokRelau berputar kelompok
Pasir KuarzaPasir Kuarza
2

Heat under nitrogen

Turn the core and bring it to temperature, usually about 975 to 1300 °C, flushing it with nitrogen before any hydrocarbon goes in.

Alatan diperlukan:

Relau berputar kelompokRelau berputar kelompok
NitrogenNitrogen
3

Crack the methane

When the temperature is steady, let in the coating gas and keep it flowing for the time needed. The film grows at a steady rate: at 1000 °C and 30 % methane the paper runs from 0.2 to 10 hours. Longer gives a thicker film of lower resistance; temperature sets the rate more than anything else, and more methane deposits faster.

Bahan untuk langkah ini:

MetanaMetana1 flow

Alatan diperlukan:

Relau berputar kelompokRelau berputar kelompok
4

Cool under nitrogen

Shut off the methane and let the core cool while oxygen-free nitrogen keeps flowing. The films come out clean, even and firmly stuck.

Alatan diperlukan:

Relau berputar kelompokRelau berputar kelompok
NitrogenNitrogen
5

Terminate the ends

Paint the ends of each coated rod with a water suspension of colloidal graphite (Aquadag), then burnish and bake it; this suits all but low-value resistors. Fit the end caps with their leads. Unknown: the caps and leads, which the paper does not describe. Ours: an agate burnisher and an oven.

Bahan untuk langkah ini:

Grafit koloidGrafit koloid1 as required
Penutup hujung perintang dengan kakiPenutup hujung perintang dengan kaki2 per resistor

Alatan diperlukan:

Penggilap akikPenggilap akik
KetuharKetuhar
6

Grind the helix

Grind a helical groove through the film with a water-cooled, metal-bonded diamond wheel, the blank floating against the wheel so the groove stays even. Pick the pitch to land slightly below the wanted value (330 Ω, 10 kΩ or any other). The groove must be smooth: cracks into the carbon ribbon bring noise and drift.

Alatan diperlukan:

Mesin pemotong heliks perintangMesin pemotong heliks perintang
7

Rub to value and varnish

Turn the resistor while measuring it continuously, and rub its whole surface lightly with a cotton pad wet with an organic solvent until it reaches its value. Leave it just below tolerance, then give it one or more coats of baking varnish, which raises the resistance by generally less than 1 %. Unknown: which varnish and its baking. Ours: acetone as the solvent, a Wheatstone bridge to measure.

Bahan untuk langkah ini:

Varnis bakarVarnis bakar1 as required

Alatan diperlukan:

Titi WheatstoneTiti Wheatstone
Kapas penyerapKapas penyerap
AsetonAseton
KetuharKetuhar

Bahan

5

Alatan Diperlukan

9

Blueprint berkaitan

Blueprint ini berkongsi pengetahuan — teknik, bahan atau prinsip

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...