Carbon Resistance Element: Lampblack in Alkyd and Chinese Wood Oil on Laminated Phenolic
A carbon resistance film for radio sets. Chicago Telephone Supply's Cooper (US 2,120,930, 1938) found that lampblack bound in phenolic resin kept drifting, so he bound it in alkyd resin modified with Chinese wood oil (tung oil). Sprayed on laminated phenolic and baked up to 165 °C, the film becomes insoluble and holds its value in heat and damp. His mix gave about 50,000 ohms in an element of ordinary size, with a film about 0.003 inch thick.
The picture: our diagram.
Pertengahan
1 day
Arahan
1
1
Make the binder: 72 alkyd, 28 wood oil
Make the binder: 72 alkyd, 28 wood oil
Mix 72 parts of alkyd resin with 28 parts of Chinese wood oil (tung oil).
Bahan untuk langkah ini:
Resin alkid Glyptal72 parts
Minyak tung28 partsAlatan diperlukan:
Neraca dua piring
Bikar Kaca
Pengacau
Sarung tangan getah2
2
Mix 25 binder, 14 lampblack, 61 solvent
Mix 25 binder, 14 lampblack, 61 solvent
Thoroughly mix 25 parts of the binder with 14 parts of lampblack and 61 parts of a solvent for the binder. The patent does not name the solvent. Ours: xylene.
Bahan untuk langkah ini:
Jelaga lampu14 partsAlatan diperlukan:
Xilena
Neraca dua piring
Bikar Kaca
Pengacau
Alat pernafasan muka penuh
Sarung tangan getah3
3
Spray onto laminated phenolic
Spray onto laminated phenolic
Spray the mixture as a thin film onto a base of laminated phenolic. The patent's film is about 0.003 inch thick.
Bahan untuk langkah ini:
Kepingan Komposit Resin Fenolik1 kepingAlatan diperlukan:
Pistol Semburan
Pemampat udara
Alat pernafasan muka penuh
Sarung tangan getah4
4
Bake: 40 °C up to 165 °C, hold 1 hour
Bake: 40 °C up to 165 °C, hold 1 hour
Put it in an oven at about 40 °C, raise the heat gradually over one hour to 165 °C and hold there one more hour. Take it out and let it cool; it is ready for use.
Alatan diperlukan:
Ketuhar pengeringan
Termometer Ketuhar
Sarung Tangan Tahan HabaBahan
4- 72 partsPemegang Tempat
- 28 partsPemegang Tempat
- 14 partsPemegang Tempat
- 1 kepingPemegang Tempat
Alatan Diperlukan
11- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- 1 vendor sell this, none ship to you yetPemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
Blueprint ini membuat
Blueprint berkaitan
Blueprint ini berkongsi pengetahuan — teknik, bahan atau prinsip

Glyptal Resin from Glycerin and Phthalic Anhydride: Callahan, 1914
oleh Charlie
Organik
30
0
0
0
0
0

Tung Oil Pressed from the Seeds of Tung Nuts
oleh Mary
Kerja Kayu
15
0
0
0
0
0

Making Lampblack Pigment — Collecting Carbon Soot from a Burning Flame
oleh Charlie
SENI
210
0
0
0
6
0

Berbahaya
Laminated Phenolic Paper Sheet: Bakelite-Coated Kraft Paper Hot-Pressed and Baked (O'Conor, Westinghouse 1918)
oleh Charlie
Industri
9
0
0
0
0
0
CC0 Domain Awam
Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.
Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.