Ceramic Disc Capacitors: Barium Titanate with Nickel Stannate, Pressed, Fired and Silvered (Coffeen, US 2,789,061)

Barium titanate with 3 mole % nickel stannate is calcined, pressed into small discs and fired hard. Silver is fired onto both faces and a lead soldered to each, giving ceramic disc capacitors of high capacity for their size. Result: discs 3/8 inch across and about 1/10 inch thick with a dielectric constant averaging 2380 and a dissipation factor of 0.58 %. Between 25 and 85 °C the dielectric constant rose at most 17 % and fell at most 7 %. Source: W. W. Coffeen (Metal & Thermit Corp.), US 2,789,061 (1957). Unknown: how the barium titanate, the nickel stannate and the tinned lead wire are made; the patent uses them ready-made. Picture: Wikimedia Commons.
Lanjutan
10 days

Arahan

1

Weigh and slurry

Weigh 19.32 g of barium titanate and 0.68 g of hydrated nickel stannate (about NiSnO3·2H2O), which is 97 mole % BaTiO3 and 3 mole % NiSnO3. Slurry them with 50 cc of distilled water. The patent prefers 2 to 4 mole % nickel stannate; 1 to 15 % works.

Bahan untuk langkah ini:

Barium titanatBarium titanat19.32 g
Nikel stanatNikel stanat0.68 g

Alatan diperlukan:

Air SulingAir Suling
Penimbang Digital JituPenimbang Digital Jitu
Piring PenyejatPiring Penyejat
2

Dry, sieve and calcine

Dry the slurry, crush it to pass a 50 mesh screen, moisten it with 5 % of a 2 1/2 % starch solution and press it into one slug. Calcine the slug for one hour at 1600 °F (871 °C). Ours: potato starch, a drying oven, mortar and pestle.

Alatan diperlukan:

Kanji kentangKanji kentang
Ketuhar pengeringanKetuhar pengeringan
Lesung dan AluLesung dan Alu
AyakAyak
Mesin tekan hidraulikMesin tekan hidraulik
Tanur suhu tinggiTanur suhu tinggi
3

Press the discs

Grind the calcine to pass a 325 mesh screen, moisten it again with starch solution, and press small discs 3/8 inch in diameter and about 1/10 inch thick at 20,000 pounds per square inch.

Alatan diperlukan:

Lesung dan AluLesung dan Alu
Ayak Bermata HalusAyak Bermata Halus
Kanji kentangKanji kentang
Mesin tekan hidraulikMesin tekan hidraulik
Acuan tekan cakeraAcuan tekan cakera
4

Fire on platinum

Fire the discs on platinum foil at 2400 °F (1316 °C) for one hour. They come out with zero absorption.

Alatan diperlukan:

Tanur suhu tinggiTanur suhu tinggi
PlatinumPlatinum
5

Silver and lead

Paint silver paint on both faces and fire the discs at 1350 °F (732 °C) for one hour. Solder tinned copper lead wires directly to the silver electrodes. Age at least a week before measuring. Ours: a fine brush and a soldering iron.

Bahan untuk langkah ini:

Cat perak bakarCat perak bakar1 both faces
Dawai kuprum bersalut timahDawai kuprum bersalut timah2 leads per disc
Dawai PateriDawai Pateri1 a little

Alatan diperlukan:

Berus berhujung halusBerus berhujung halus
Tanur suhu tinggiTanur suhu tinggi
Alat pematerianAlat pematerian

Bahan

5

Alatan Diperlukan

14

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...